Thanks to Mr John A. Henning who has given clear cut answere as per code.

Pandithan
Welding consultant


On Thu, May 23, 2013 at 9:44 PM, John Henning <jhenning@deltak.com> wrote:

The WPS must reference the supporting PQR. 

 

However, The PQR does not have to reference any WPS.  You may reference a WPS if that is something you want to do.

 

As stated by others, a single PQR may support a multiplicity of WPS's.  In that case do you require all WPS's supported by the PQR to be referenced on the PQR?  Stuff and nonsense. 

 

Obviously you will have a trial "WPS" or set of instructions for the welder  stating the starting parameters or parameter ranges.  You are not required to retain or present this with your WPS.  By extension you would not have to "name" this trial document. 

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of SRINI
Sent: Thursday, May 23, 2013 8:24 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:17774] WPS no. on PQR

 

Dear Kanagapandian

 

It shall be mentioned in PQR.

 

Please go to caluse QW-200.1 (b) & (e)second paragraph

 

The WPS shall reference the supporting Procedure Qualification

Record(s) (PQR) described in QW-200.2. The

manufacturer or contractor may include any other information

in the WPS that may be helpful in making a Code.

 

(e) Availability of the PQR. PQRs used to support WPSs

shall be available, upon request, for review by the

Authorized Inspector (AI). The PQR need not be available

to the welder or welding operator.

 

PQR- is  only one time

WPS-  we prepare many time with in essential limit in supporting PQR. 

 

On Thu, May 23, 2013 at 5:22 AM, John Henning <jhenning@deltak.com> wrote:

No, it is not required.    See QW-200.2 (b) – Contents of the PQR.  "The completed PQR shall document all essential and , when required supplementary essential variables of QW-250 through QW-280 for each welding process used during welding of the test coupon.  Non-essential and other variables used during the welding of the test coupon may be recorded at the manufacturers or contractors option.  . . . "  There is no requirement for recording a WPS number.

 

Further, regarding the form provided by Sc IX " Form QW-483, see Nonmandatory Appendix B, has been provided as a guide for the PQR.  . . ."

 

See also the last paragraph of QW-100.1 "The PQR documents what occurred during welding the test coupon and results of testing of the coupon.  As a minimum, the PQR shall document the essential variables and other specific information identified in Article II for each process used during welding the test coupon and the results of the required testing.  In addition when notch toughness testing is required for procedure qualification, the applicable supplementary essential variables for each process shall be recorded."

 

For ASME Section IX it is NOT required.   

 

When stating requirements, one should provide Code reference(s) otherwise indicate it is an "opinion".

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of james gerald
Sent: Thursday, May 23, 2013 2:15 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:17760] WPS no. on PQR

 

Yes it is required.

 

 

 

Thanks & Regards

J.Gerald Jayakumar
00968-99438165

From: kannayeram gnanapandithan <kgpandithan@gmail.com>
To: materials-welding@googlegroups.com
Sent: Thursday, May 23, 2013 8:43 AM
Subject: [MW:17758] WPS no. on PQR


Is it required to put WPS no. in PQR, if so pl give code ref
Pandithan
Welding Consultant

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...