Skip to main content

Re: [MW:17754] Impact test- minimum thk requirement

Thanks Gents.
It is very clear that impact test shall be performed up to 2.5mm thk.
 
Appreciate all your valuable guidance.
 
Best Regards,
Victor.

On Thu, May 23, 2013 at 6:51 AM, kannayeram gnanapandithan <kgpandithan@gmail.com> wrote:
2/3 of 27 joules is also acceptable in some codes
Pandithan
welding consultant

On 5/22/13, Ramin Kondori <raminkondori@gmail.com> wrote:
> *Dear Victor:*
>
> In our project we have similar requirements for Duplex and Super Duplex as
> James mentioned (regardless of thickness) where it requires impact test at
> -46 degC and results should demonstrate average of minimum 27J and no
> result less than 20J).
>
> Regards
> *Ramin Kondori*
> *Sr. QA/QC Engineer
> *
> *SINOPEC*
>
> r.kondori@petroyada.com
> +98-2123592322
> +98-9132150320
>
>
> On Wed, May 22, 2013 at 3:24 PM, james gerald <gerry_tup@yahoo.com> wrote:
>
>> Impact test not required/cannot be performed if the thickness is below
>> 2.5mm.
>>
>> Check with Metallurgy Lab whether they can machine your sample with
>> thickness 3.73mm and perform Impact.
>>
>> If yes, then Impact test need to be performed at -46/-50degC for Duplex.
>>
>> Thanks & Regards
>>
>> J.Gerald Jayakumar
>> 00968-99438165
>>    *From:* victor george <dvgeorge@gmail.com>
>> *To:* materials-welding@googlegroups.com
>> *Cc:* Arul prakash <r.arulprakash@gmail.com>
>> *Sent:* Wednesday, May 22, 2013 2:33 PM
>> *Subject:* [MW:17738] Impact test- minimum thk requirement
>>
>> Hi Experts,
>>
>> Please explain what is the minimum thickness requirement of impact test.
>>
>> Material: A790 S31803 pipe
>> Size: 1/2' Sch 80 (WT- 3.73mm)
>> Sour service
>>
>>
>> Question: Is it possible to do impact test on 3.73 thk?
>>
>>
>> Best Regards,
>> DV.George
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>>
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views
>> and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>> ---
>> You received this message because you are subscribed to the Google Groups
>> "Materials & Welding" group.
>> To unsubscribe from this group and stop receiving emails from it, send an
>> email to materials-welding+unsubscribe@googlegroups.com.
>> For more options, visit https://groups.google.com/groups/opt_out.
>>
>>
>>
>>
>>   --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>>
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views
>> and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>> ---
>> You received this message because you are subscribed to the Google Groups
>> "Materials & Welding" group.
>> To unsubscribe from this group and stop receiving emails from it, send an
>> email to materials-welding+unsubscribe@googlegroups.com.
>> For more options, visit https://groups.google.com/groups/opt_out.
>>
>>
>>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...