Friday, November 25, 2011

Re: [MW:13053] PTC Requirement for S.S.

Dear Vijay,

In general to decide Production coupan plate requirement  procedure are

PTC requirement mention in UG-84 and those requirement are further waived for specific material in relevant subsection of the code i.e.   UCS- 67, UHA 51, UHT-87

and if welding procedure required impact test then it not mandatorily required PTC in all case.

For easy interpretation of UHA-51 for impact test requirement refer Non Mandatory appendix JJ of ASME Sec VIII Div.1

In your case if considering  Welding by GTAW , SMAW or SAW

Impact test for Base Material & HAZ : Not Required
Pre qualification of filler material : Required
Impact test for WPS qualification: Required.
Production test coupan : Not required



Best Regards

Rajesh Patel
Executive Engineer  - Materials Technology, QA/QC & Standards




From:        Vijay Katkar <katkar.vijay22@gmail.com>
To:        materials-welding@googlegroups.com
Date:        24/11/11 21:59
Subject:        Re: [MW:13046] PTC Requirement for S.S.
Sent by:        materials-welding@googlegroups.com




Dear Rajesh,
 
My confusion, impact test is required for welding procedure qualification as per UHA-51(e) and weld metal (UHA-51f) also. Only base metal and HAZ is exampted as per UHA-51. if welding procedure required impact test then we need to have PTC for the job as per UHA-51 h..
 
Am i right or UHA-51 saying somthing different. please confirm...
 
Regards
 
Vijay Katkar 

On Thu, Nov 24, 2011 at 6:41 AM, <Rajesh.Patel@linde-le.com> wrote:
Dear Vijay

If welding is performed with the use of filler material up -196 deg C, Production Test Coupan is not required.

for PTC requirements refer UHA 51 h


Best Regards

Rajesh Patel
Executive Engineer  - Materials Technology, QA/QC & Standards





From:        
Vijay Katkar <katkar.vijay22@gmail.com>
To:        
materials-welding@googlegroups.com
Date:        
23-11-11 21:44
Subject:        
[MW:13040] PTC Requirement for S.S.
Sent by:        
materials-welding@googlegroups.com





Dear All,
 
I have one vessel with M.D.M.T -140 Degree C. for base metal (SA 240 TP 304) impact test is exampted as per UHA 51 Of ASME section VIII Division- 1 but consumable and procedure qualification impact test is required as UHA-51 ,
PTC is required for vessel with above condition, please advice .........
 
 
Regards
 
Vijay Katkar

--
To post to this group, send email to
materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to
materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...