Re: [MW:4769] Multiple PQRs for Impact test requirement

Dear Ibrahim,
 
please find attachment for Impact test requirement code interpretation.
 
Regards,
S.veloumany


From: Muhammed Ibrahim <ibratech@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wed, April 7, 2010 6:59:29 PM
Subject: Re: [MW:4744] Multiple PQRs for Impact test requirement

 
Dear Sir,
 
As per the below statement QW 401.3  & ASME Interpretations IX-04-04 the base metal will support from 6 to 200?.

"When essential variables are qualified by one or more

PQRs and supplementary essential variables are qualified

by other PQRs, the ranges of essential variables established

by the former PQRs are only affected by the latter to the

extent specified in the applicable supplementary essential

variable (e.g., essential variable QW-403.8 governs the

minimum and maximum thickness of base metal qualified.

When supplementary essential variable QW-403.6 applies,

it modifies only the minimum thickness qualified, not the

maximum)."


On 6 April 2010 11:25, <george.dilintas@gr.bureauveritas.com> wrote:

Hi,
Regarding individual (SMAW and GTAW) T limits what are you saying complies with QW-403.6, but you can not club those two PQRs and lower the T limit.
T is not the deposited weld metal thickness but the global (total) thickness.
I think in case you want to have a qualified WPS valid from 6 to 200 mm this is not possible when impact test is required.
UCS 67 does not give any exemption related to the type of the weld (A or B or D...) and the production impact test (UG084(i)) is not to be confused with the
WPS qualification


Dr. G. Dilintas
I&F Regional Technical Manager
Bureau Veritas Piraeus - Greece
Tel: +30 210 40 63 113/4
Fax: +30 210 40 63 118
Inactive hide details for Muhammed Ibrahim <ibratech@gmail.com>Muhammed Ibrahim <ibratech@gmail.com>



To

materials-welding@googlegroups.com

cc


Subject

[MW:4648] Multiple PQRs for Impact test requirement

Ref


 
Hi Members,
 
Please provide a solution for the following issue.
 
Shell Material : SA 516 Gr.70 -- 50 mm Thk
Nozzle : SA 333 Gr.6 --- 7 mm thk
 
MDMT : - 46 Deg.C
 
I need to weld the nozzle to shell. I have a PQR with SMAW process qualified in 40 mm thk and another PQR with SMAW qualified in 6 mm thk.
 
As per Sec. IX if impact test is required the 40 mm PQR will support from 16 mm to 200 mm. base metal Thk. and the other PQR will support from 6 mm to 12 mm thk.
 
If I club these PQR can I write a WPS to support 6 mm to 200 mm?.
Is there any issue for the missing range of qualification between 12 mm to 16 mm?.
Or is it required to add another PQR to fill the missing thickness range from 12 to 16 mm between the first two PQRs?.
Or can I write a WPS directly with range 5mm to 200mm omiting impact test requirement for this joint as it is a category D joint and excempted from Production Test Coupon?.

Thanks & Regards
Muhammed Ibrahim PK

--

To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Thanks & Regards
Muhammed Ibrahim PK

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...