[MW:24376] RE: 24374] RE: 24373] Time between Hydrogen Bake Out and PWHT

Once our shop got a relax from client to keep it as long as one week if the storage was done with assurance that relative humidity would be low and not create risk of cracking due to water.

What we did during that time was using heater in storage shade and monitoring humidity.

Anyhow,  no body is comfortable to see 15E welded joint stayed without PWHT too long.  PT/MT and volumetric inspection after PWHT is highly recommended.

Regards,

C.Nopadon

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pgoswami
Sent: Friday, February 26, 2016 11:59 AM
To: materials-welding@googlegroups.com
Subject: [MW:24374] RE: 24373] Time between Hydrogen Bake Out and PWHT

 

Hi Mac,

 

One week without PWHT on 3.5" think Grade -91 Steel is too long. In spite of hydrogen bake out one may get cracking. Did any one check the hardness of weld and HAZ by any means (just for curiosity??).

 

Also prior to the DHT the welds should be cooled to Mf   temperature which is generally  the ambient temperature. In absence of it full martens tic transformation won't happen causing poor creep strength in these steels. DHT may be adopted before the PWHT, however not advised to delay PWHT so long.

 

It's worth looking at.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgoswami@quickclic.net

pradip.goswami@gmail.com

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com]
Sent: Thursday, February 25, 2016 3:47 PM
To: Materials & Welding
Subject: [MW:24373] Time between Hydrogen Bake Out and PWHT

 

Dear Sirs,

We welded a 15E Pipe material (16 inch - 87mm thickness).
Our procedure will be preheated with 205 deg centigrade then welding and will be
( hydrogen ) bakeout and perform PAUT, If accepted in PAUT, immediately followed
by PWHT and will perform MT.
Process is B31.1

The joint has been accepted by PAUT, my query is, how long should be acceptable if there is a delay in performing PWHT?
Right now it is almost 1 week that the welded joint is not yet PWHT.

Need your advice.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2273403b-7345-464c-8e91-93d53134f4f8%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAYAAAAAAAAAOT5XfyRhstKvyeqQRSrfFXCgAAAEAAAAClD1TdHQKRLquEJzyVMUawBAAAAAA%3D%3D%40quickclic.net.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...