[MW:20837] RE: 20835] Re: Delta Ferrite Test on SS 316L

Hi Sandeep,
 
SS 316L casting would always contain some ferrite, in cast condition.See the attached document for general guideline. This is an extract from NIDI publication document -11022. The easiest way to get round this issue would be to perform solution anneal, after casting.
 
Ferrite determination is performed either by Ferrite Scope, the readings expressed in Ferrite No (FN) or Volume Percentage Ferrite calculation as per ASTM E-562. Schaffler-Delong diagram is quite accurate to  predict ferrite in weld metal. This may not be always true for cast or formed components. Ferrite in austenitic stainless steel is a high temperature precipitation phase.
 
The only way to get "Zero" ferrite would be to balance the composition , by introducing "Nitrogen " in the melt over and above the required other alloying elements, e.g Cr,Ni & others. At the same time components must be solution annealed following casting and rough machining. Final machining may follow solution anneal.
 
Hope this clarifies your query.
 
Thanks
 
 
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
pradip_goswami@yahoo.ca
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Sandeep Sandeep
Sent: Saturday, May 17, 2014 1:00 PM
To: materials-welding@googlegroups.com
Cc: rudolf saldanha; c sridhar
Subject: [MW:20835] Re: Delta Ferrite Test on SS 316L

Dear Sir

We are the casting manufacturer of Orthopedic Item in SS 316L. We are facing some problem of Delta ferrite. Our customer required 100% ferrite free material. Pleas sir can you pleas help us how we can reduce our ferrite. Currently our ferrite is coming aroung 10%. and what is the best method of ferrite testing.


Waiting for your valuable reply.


Regards


Sandeep
8003294160




On Tuesday, 15 January 2013 10:44:52 UTC+5:30, sridhar wrote:
Mr. Rudolf,

Please refer to your mail and shall answer your following queries to the best of my knowledge and in a short form. 
No apologies as we  all help each other in one form or other. If you need more info. please feel free to write  to us.

Query:
One of the clients requirement is that Delta Ferrite has to be checked on the weldment as per Schaeffler method.

1. what is this delta ferrite test & how is it conducted
 
a)To understand it, one has to know reason for ferrite formation. Welding metals like 304L, 316L, retain some
amount of delta ferrite formed at grain boundaries, due to composition of weld metal & welding conditions like
high temperature (5500 - 9500C). Both factors determine the percentage of delta ferrite as well as its size,
morphology and distribution. Though delta ferrite reduces risk of micro fissuring / cracks, if it exceeds 8-10%, corrosion resistance of SS decreases steeply. Ferrite level beyond 7% is unacceptable for high temperature service. Again, Zero or very low ferrite may also create micro-fissures. Hence it has to be checked  /inspected depending
up on theservice conditions.

Ferrite turns to brittle sigma phase (rich in Cr)  at high temperature and affects ductility, toughness and also cause  inter granular corrosion due to Cr depletion from austenite matrix. Hence it has to be maintained depending up on service requirements.

These details were brought by Schaeffler by metallographic  i.e., Ferrite Percentage (shown in the annexure) 
which helps to determine the structure of weldment, like ferrtic, austenitic , percentage of delta ferrite at normal conditions etc. The limitation is the non-equilibrium cooling rate, selection of welding process, shielding gas,
non inclusion of Nitrogen (a strong austenite former)  which has influence on the ferrite morphology. 

De-long has modified the Schaeffler diagram (claimed to be ±4% accurate) improving the accuracy to ± 2%. 
De-long diagram differs with Schaeffler diagram as the  that the values are based on magnetically determined
ferrite content. i.e., the Ferrite No & Nitrogen is included in the calculation of nickel equivalent with a coefficient equivalent of 30.
 
Hence it generally believed that, De-long diagram gives more accurate values compared to Schaeffler diagram.
AWS has switched over to Ferrite No. (FN) instead of percentage ferrite since, FN is derived by a standard measurement and calibration procedure as approved by Welding  Research Council
 
2. Do we buy the instrument and do it ourselves or hire a ndt service company to do this.
   what does this test mean and what does it say.   Is it a destructive test or NDT.   Can we do a PMI and work out
   the Ni (eq) or Cr (eq) to arrive at the Ferrite No. What is the unit of the Delta Ferrite.

a) In Schaeffler diagram, Nickel and Chromium equivalents are calculated and Delta Ferrite percentage is obtained by plotting the values. (Cr Equiv.: % Cr + % Mo + 1.5 % Si + 0.5%Cb  & Ni Equiv. : % Ni + 30% C + 0.5% Mn)
This method involves actually counting the ferrite phase using point counter method and estimating the percentage)
 
In De-long  diagram the Delta Ferrite No.  i.e., FN  is calculated by adding additional 30% N in Ni equiv.)
 
These method is based upon the theory that, ferrite is a magnetic phase in a non magnetic austenitic matrix.

While Nitrogen level in SMAW is 0.06%,  it is 0.02% through GTAW &  0.04% in GMAW process.
 
Magnetic saturation method is a DT to determine the absolute percentage of delta ferrite in the sample and
independent of size, shape, orientation of  the phase etc. Cannot be used to measure ferrite in an actual equipment.
 
Ferrite scope, Magna gauge are other methods, to measure the delta ferrite and their results are said to be accurate and widely used due to its simplicity. They are NDT methods and could be used any one. Both gauges are available easily in the market. No need to have a service company (can be done by yourself) if the no. of checking are frequent and on a long run. 
 
Other  special methods used in a research institute are X-ray diffraction, Electro chemical  etc.
 
Schaeffler and De-long Diagrams are given in the annexure.
 
Trust above information, gathered from various references shall be of help to you.
 
Sridhar.
                                                      




<w:LsdException Locked="false" Priority="64" SemiHidden="false" UnhideWhenUsed="false" Name="Medium Shading 2 Acce
...

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...