Skip to main content

Re: [MW:20610] WPS as per API 650

BEGIN:VCARD
X-LOTUS-CHARSET:UTF-8
VERSION:3.0
PRODID:-//Lotus Development Corporation//NONSGML Notes 8.5.2//EN_C
FN:George H Dilintas/GRC/VERITAS
N:Dilintas;George;;;
ADR;TYPE=WORK;TYPE=PREF:PIRAEUS;;23\, Etolikoy Str.;PIRAEUS;;185 45
;GREECE
ADR;TYPE=HOME;TYPE=PREF:;;19-21 B. Laskou str.;Athens;Attika;11 633
;Greece
TEL;TYPE=HOME:+30-1-7667 197
TEL;TYPE=WORK:+30-210-40 63 113
TEL;TYPE=HOME;TYPE=FAX:+30 - 1 - 7667 197
TEL;TYPE=WORK;TYPE=FAX:+30-210-40 63 118
TEL;TYPE=CELL:+30 -69 44-64 62 04
EMAIL;TYPE=WORK;TYPE=PREF;TYPE=INTERNET
:george.dilintas@gr.bureauveritas.com
ORG:Bureau Veritas;Industry
REV:20131201T024559Z
END:VCARD

If Thermal Stress Relief (PWHT) is not required by API 650, then you have not to perform a PWHT on your PQR specimen

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor
    API 510 Inspector

    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    (See attached file: Dilintas_George.vcf)

Marat Nurbekov ---16/04/2014 15:56:42---HI Dear Members, Could you help me? I work in project for Crude Oil Tank. The tank shall

From: Marat Nurbekov <marat.nurbekov@gmail.com>
To: materials-welding@googlegroups.com
Date: 16/04/2014 15:56
Subject: [MW:20597] WPS as per API 650
Sent by: materials-welding@googlegroups.com




HI Dear Members,
Could you help me? I work in project for Crude Oil Tank. The tank shall be constructed as per API650 and now I have some following doubts:
1) As you know WPS for API 650 has to be qualified as per ASME IX CODE and as per this code PWHT is essential variable but what about Thermal Stress Relief which is required as per API 650?
Shall I qualify WPS with Thermal Stress Relief or Thermal Stress Relief shall be performed when it is required as per API 650
2) For Crude Oil Tank shall be constructed Fire water pipe system and Drainage system. Company is going to use a plastic pipe material but there are not any notes regarding plastic materials in ASME IX and API 650.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .