Skip to main content

Re: [MW:16532] Using of ER70S-6 in place of ER70S-2


On special request and order, consumable manufacturer can provide ER 70S-2 in spool form.
I have used ER 70S-2, size: 1.2mm in spool form for automated TIG applications in past.
 
Regards
 
Prem Nautiyal
9769316004

--- On Wed, 1/16/13, kannayeram gnanapandithan <kgpandithan@gmail.com> wrote:

From: kannayeram gnanapandithan <kgpandithan@gmail.com>
Subject: Re: [MW:16531] Using of ER70S-6 in place of ER70S-2
To: materials-welding@googlegroups.com
Date: Wednesday, January 16, 2013, 8:20 PM

As per code, Minimum tensile value is 70000psi. It is not as stated in
the trailing mail. I do not think that ER70S2 is available in spool
and hope that manufacturer of welding consumable who are in this forum
may give their comments pl
Pandithan
Welding consultant


On 1/12/13, nithindsilva4u@gmail.com <nithindsilva4u@gmail.com> wrote:
> Hi,
>
> ER70S-6 has a higher mangnaese and silicon content giving this rod better
> tensile strength and smoother running characteristics then ER70S-2. Tensile
> strength is up to 88,000 psi. ER70S-2 is a triple deoxidized mild steel rod
> which will give quality welds on most grades of steel. Tensile strength if
> 77,000 psi.  Both are available in rod (GTAW) as well as spool form (GMAW).
> With respect to ASME Section IX, when using in place ER 70S-2, b sure u r
> checking the A No. of ER 70S-6, as sometimes the chemical composition
> varies. if its matching then you can use.
> --
> regards,
> Dsilva
>
> Sent from my iPhone
>
> On Jan 11, 2013, at 9:17, kannayeram gnanapandithan <kgpandithan@gmail.com>
> wrote:
>
>> Can be used provided if it is available in rod for TIG process.
>>
>> Generally ER70S2 comes in rod form for TIG welding not in spool form for
>> GMAW process because in GMAW process, Titanium gets oxidided in arc itself
>> and purpose of Ti adding is lost, so it is not at all used in GMAW
>> process.
>>
>> ER70S6 comes generally in spool forms for GMAW process and if it comes in
>> rod, it can be used in TIG process
>>
>> Pandithan
>> Welding Consultant
>>
>> On Thu, Jan 10, 2013 at 7:48 PM, c sridhar <sridhar305@yahoo.com> wrote:
>>> Mr. Chakraborthy,
>>>
>>> You have not given  the  process details. Is it MIG or TIG process.
>>>
>>> In general:
>>>
>>> For TIG process, we use ER 70S-2 for CS welding. The shielding gas used
>>> will be Argon. Radio graphic
>>> quality is assured due to addition of Ti, Zn & Al which removes Oxygen
>>> by forming faster oxides with it
>>> along with Mn.& C. ER 70S-6 is available in spool form ( 15 kg  or so)
>>> and not used for TIG process as it
>>> can not provide X-ray quality welds
>>>
>>> For MIG process, ER 70S-6 is generally used with  Carbon-DI-oxide as
>>> shielding gas. ER 70S-6 has
>>> excessive Mn & Si  (1.85 & 1.15 %  respectively) compared to 1,4 & 0.7 %
>>> in ER 70S-2 filler wire,
>>> Additional Mn, & Si will remove oxides form CO2 gas to give good weld
>>> quality, but consistency to
>>> provide x-ray quality is a question mark. ER 70S-2 could also be used
>>> but, only with Argon gas.
>>>
>>> Sridhar.om: Ranendra Chakraborty <ranendrac6@gmail.com>
>>> To: materials-welding@googlegroups.com
>>> Sent: Thursday, 10 January 2013 12:13 PM
>>> Subject: [MW:16480] Using of ER70S-6 in place of ER70S-2
>>>
>>> Dear Expert,
>>> Please guide whether ER70S-6 can be used in place of ER70S-2. Please give
>>> code reference.
>>>
>>> Regards,
>>> Ranendra
>>> --
>>> To post to this group, send email to materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
>>> materials-welding+unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>>
>>> The views expressed/exchnaged in this group are members personel views
>>> and meant for educational purposes only, Users must take their own
>>> decisions w.r.t. applicable code/standard/contract documents.
>>>
>>>
>>>
>>>
>>> --
>>> To post to this group, send email to materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
>>> materials-welding+unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>>
>>> The views expressed/exchnaged in this group are members personel views
>>> and meant for educational purposes only, Users must take their own
>>> decisions w.r.t. applicable code/standard/contract documents.
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>>
>>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>
>
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...