Skip to main content

RE: [MW:16374] SENSITIZATION OF STAINLESS STEEL.

Vinu,
 
ASTM 262 is the industry followed standard  for intergranular corrosion test. This standard  is divided  into 5 test categories:-
  • Practice A- Oxalic Acid  Etch Test for Classification of Etch Structures .
  • Practice B—Ferric Sulfate–Sulfuric Acid Test for Detecting Susceptibility to Intergranular Attack

  • Practice C—Nitric Acid Test for Detecting Susceptibility to Intergranular Attack

  • Practice E—Copper–Copper Sulfate–Sulfuric Acid Test for Detecting Susceptibility to Intergranular Attack

  • Practice F—Copper–Copper Sulfate–50 % Sulfuric Acid Test for Detecting Susceptibility to Intergranular Attack

The best screening for sentization is possible by Practice -A test. Usually a presence of "Ditched microstructure" is an indication of sensitization. You may please contact an experiences laboratory for further deatils.
 
Thanks.
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 
 
Please ignore my earlier email as the spell check was not properly done. 

From: Vinu Raveendran <vinuravi007@gmail.com>
To: materials-welding@googlegroups.com
Sent: Saturday, December 29, 2012 11:49 AM
Subject: [MW:16359] SENSITISATION OF STAINLESS STEEL.

Dear Member,

How can i detect or find out if a stainless steel material is sensitised or not.?
 Is there any tests to find sensitisation of ss?codes?

Thankyou!

--
VINU RAVEENDRAN
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .