Saturday, November 26, 2011

Re: [MW:13063] Welding of AISI 316L to A516 Gr B regarding

Just 309 is ok. 316 with carbon steel will give hot cracks because of low FN. You need a filler metal with much higher Cr and Ni content to avoid low FN
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: Eswaran samikannu [eswaranaws@yahoo.co.in]
  Sent: 26/11/2011 12:54 ZE5B
  To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
  Subject: [MW:13062] Welding of AISI 316L to A516 Gr B regarding



Good day to all,
Please refer the attachment  for joint configuration, I have to qualify the procedure for AISI 316L to A516 Gr B steel
Thickness of the job maximum 64 mm. I proposed to use 35 mm thickness plate for qualification.Code requirement ASME Sec IX
My plan as follows
1) Buttering the Bevel area of A516 Gr B material using E 309 consumables up to 3 to 5 mm
2) Machining of Bevel & PT (NDT) & Fit up
3) Welding of A516 Gr B to to AISI 316L using E316 consumables 

Kindly  advice me what preheat temperature  & Interpass temperature can maintained during welding, Any PWHT required or not,any other precautionary measures during welding & mechanical testing.
My client not specified anything. Please someone advice to me.
Thanks
Regards
E.Jegan  