Wednesday, April 28, 2010

Re: [MW:4990] API 5L X85 -CVN Requirements

Mr. K. Babu:
 
API 5L ,ed. 44, does not request longitudinal CVN test, because due to rolling process for plate production for seam weld pipe or seamless pipe, the grain orientation of the microstructure has the lowest  fracture toughness values  transverse to pipe axis. Therefore, CVN spicemens must be taken transverse to the pipe axis based on the fact that this is the most unfavorable spicemen orientation to obtain the minimum requested absorbed energy values
On the other hand, X85 grade is an intermediate grade agreed for production between purchaser and manufacture
According to table 8 of API 5L, for body full size absorb energy the values for X85 grade can be interpolated according to values for grades X80 and X90 which is 30 ft-lb for pipe diameters from 20 to 36 inches and for test temp of 0°C (32°F), or lower temperature if agreed.
 
For CVN test for seam weld and H.A.Z., according to 9.8.3, the absorb energy value is also 30 ft-lb at 0°C (32°F), or lower temperature if agreed.
 
Carlos Quintini
Quintini Consultores C.A.
Venezuela

2010/4/28 Kathalingam Babu <kathalingam.qaqc@ppl.com.sg>
There is an intermediate grade called API 5L X85 , it is commonly used in offshore industries.
 
Might be added in next edition of API 5L Spec.
 
Sent: Wednesday, April 28, 2010 4:17 PM
Subject: RE: [MW:4973] API 5L X85 -CVN Requirements

I heard that 44th edition of API 5L has 3 new grades X90, X100 and X120.
what is X85? CVN is mandatory for all PSL2 pipes, refer para 6.2.5.2


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kathalingam Babu
Sent: Tuesday, April 27, 2010 3:53 PM
To: materials-welding@googlegroups.com
Subject: [MW:4966] API 5L X85 -CVN Requirements

Gents,
 
Pls tell me, what is the CVN (Longitudinal) Requirements for the API 5L X85 (19 mm thick) ?
 
Thanks & Regards,
 
K.Babu


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35738] ASME IX WPS Qualification Query: GTAW + FCAW with Multiple PQRs

Dear Welding Experts, I'm currently preparing a Welding Procedure Specification (WPS) and have encountered a request to qualify a GTAW +...