Hi, Rui,
Fortunately, I am working in Boehler Welding China Representitive.
please find enclosed paper sheet of both T-PUT and Boehler products. It may help you I think.
My fellows and I discuss your case, our commends are:
1, the diameter is OK. there is no difference between 1.0 and 1.2mm in welding.
2, you have to control interpass temperature. commonly, ≤150℃ is requested, but we prefer to ≤120℃.
3, pre-heating is not necessary.
4, low heat input!
I hope it will help you.
Regards
Roy LIU
To: materials-welding@googlegroups.com
Subject: [MW:4958] Super Duplex Welding
From: Rui.Pinho@pt.linde-gas.com
Date: Mon, 26 Apr 2010 12:45:47 +0100
Dear All
We have problems for welding Super Duplex Nº 1.4410 (see attach of Base Material Certificate) with8 mm thickness.
The process is GMAW - MAG welding an use wire electrode AWS A5.9-06 : ER2594 (see attach of Wire electrode Certificate) and the shielding gas is Ar+20%He+2%CO2
The bead of first pass is OK, but the next pass (interpass) have lots of porosity, no penetration and Spatter.
Will be control the temperature of interpass?
Will be change the wire electrode?
Thanks for help
Best Regards
Rui Fernandes Pinho
Divisão de Gases Industriais
Desenvolvimento de Aplicação de Gases
Linde Sogás, Lda.
Travessa Joaquim Dias Salgueiro, Nº 44
4470-416 Vila Nova da Telha, Portugal
Phone + 351 22 999 8380, Fax: + 351 22 996 4039
Mobile + 351 91 473 9197
rui.pinho@pt.linde-gas.com, www.linde.pt
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
更多热辣资讯尽在新版MSN首页! 立刻访问!
Subscribe to:
Post Comments (Atom)
[MW:35692]
Dear all Can I do MPI above painting surface for cs tank Regards, Sriram Srinivasan -- https://materials-welding.blog...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-