[MW:3380] RE: 3366] Re: R: 3364] Re: R: 3361] Re: Heat Input

Jeremy,
 
I agree with you.  It is common pipeline practice in the both the US and Canada to put in a root with E6010 and fill the joint with 7018.  If only the root is made with 6010 the deposit thickness will generally be less than 3/16 in. (5mm) thick.  The subsequent pass with 7018 will consume nearly the entire root pass (if it doesn't melt through).  I have seen impact test specimens removed from the root area of the weld and they have passed -20F (-30C) easily.  The reality is that the root will have acceptable properties at reasonably low temperatures.  Although, it may be important to note that pipe line welds may not be as heavily loaded as other applications.  In severe conditions GTAW would be a better process, as crack initiation will become a more critical factor and elimination of any preferential material is desireable.  But practically, it is one hell of a lot easier in the field to use SMAW than GTAW (not to mention less expensive).  That, combined with successful application of this type of weld over the past 30+ years, is why this process is still employed.
 
I have my doubts about the use of any low hydrogen SMAW electrode for open root welding.  I have seen and tested weldors with E7018 open root (very good weldors) and they have passed RT and bends, but I would not want most weldors doing this.  Because of the slag type associated with low hydrogen electrodes you open yourself up to serious weld flaws.
 
I would disagree that European industry is more advanced.  There are just differences in approach to the same problems with one side of the pond being more conservative in some areas and the other side more conservative others.  Both sides have had significant problems due to their particular type of tunnel vision.  While there is a lot of cooperation between Canada and the US, they have their individual ways also, e.g. CWB regulations for structural welding and local provincial requirements.  Canda has representatives on many US welding committees such as AWS A5 and ASME B&PV Code and I know from personal expereince that their expertise/opinions are well respected. 
 
John


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Jeremy Zibin
Sent: Tuesday, September 29, 2009 5:10 AM
To: materials-welding@googlegroups.com
Subject: [MW:3366] Re: R: 3364] Re: R: 3361] Re: Heat Input

I was never involved with qualifying the WPS using these methods and I have only observed these procedures being used widely in industry.  From what I recall, the impact specimens were cut from the full weld section so the results would show mech. properties from both the root and fill combined (both 6010 & 7018) and they passed for qualification.  I do not believe there was testing performed soley on the root pass as this thickness would not provide enough materials for a specimen.
 
I agree with you that welding technologies & consumables have evolved over the past decades and there are higher quality options available today.  My whole point was that this type of welding using 6010 & 7018 is currently being used at construction sites and on pressure piping under ASME B31.1 .   Keep in mind that Canada's welding & construction is dominated by American standards and practices, so this may be one reason why these practices are still in use versus the European industry which is more advanced.  I'm not saying which is a better option, just that this type of WPS is an option and is being used today.
 
JZ

--- On Tue, 9/29/09, Cotzia Francesco <Francesco.Cotzia@saipem.eni.it> wrote:

From: Cotzia Francesco <Francesco.Cotzia@saipem.eni.it>
Subject: [MW:3365] R: 3364] Re: R: 3361] Re: Heat Input
To: materials-welding@googlegroups.com
Received: Tuesday, September 29, 2009, 2:43 AM

Jeremy,

 

We can play with the dilution as much as we want. Have you tested the root pass only or not?

20 years ago, there was no such knowledge on this subject as today. During this period, it has been done also several damages. It is not a good point to say: "it has been done like this for several years and we have to follow the same way".

I'm not talking about GTAW only but you can use for the root pass some semi-basic electrode that can guarantee quality and productivity in the same time.

Bear in mind that if we are talking about pipeline, today there is no code where you can use cellulosic electrode for the root pass.

 

This is my point of view that as far as I can understand, it is different from yours.

 

Regards

 

F

 

 


Da: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Per conto di Jeremy Zibin
Inviato: martedì 29 settembre 2009 10.43
A: materials-welding@googlegroups.com
Oggetto: [MW:3364] Re: R: 3361] Re: Heat Input

 

Francesco,

 

I agree that the cellulosic electrode is problematic for low temp. applications, especially for danger of H2 cracking.  There is usually tight quality control on the electrodes and they are always in rod ovens prior to use.  Also, the root pass is limited in thickness, 5 or 6mm if I remember properly on the WPS, applied with a small diameter electrode.  The second pass (7018) or hot pass is applied immediately after the root pass and it blends in with the root pass and thus creates a mixture of 6010 & 7018 in the root (i.e. the root is not totally 6010 in mech. properties).

 

I'm just adding to the discussion what I've observed in the oil & gas industry in Canada.  The welding with 6010 & 7018 for LTCS is quite common and it is approved from very large clients at multi-billion dollar sites that have been in operation for 20 years or more, so I would think these people know their welding, especially in the cold temperatures of Northern Canada where it is not uncommon to see -50 or -60C during the Winter.

 

Of course a GTAW root would be of higher quality and shouldn't have any issues with low impact resistance but this process is impractical/uneconomical for production welding on construction sites where manual welders are welding hundreds or thousands of pressure piping joints everyday.  Not to mention, you would have trouble finding enough welders that could TIG roots on these large construction sites in the oilsands.

 

Regards,

 

JZ 

--- On Tue, 9/29/09, Cotzia Francesco <Francesco.Cotzia@saipem.eni.it> wrote:


From: Cotzia Francesco <Francesco.Cotzia@saipem.eni.it>
Subject: [MW:3363] R: 3361] Re: Heat Input
To: materials-welding@googlegroups.com
Received: Tuesday, September 29, 2009, 1:13 AM

Jeremy,

 

The use of cellulosic electrode for low temperature carbon steel is not quite appropriate. Sometimes and especially nowadays there some product classified as E6010 that can bear CVN at -46°C. I don't know the diameter of root pass electrode, the WT you have used for PQR nipple, but I think that the weld metal deposited by cellulosic electrode is not more than 2mm. When you are extracting the CVN specimens, you will never test them the root pass. Then you are not sure that the E6010 will resist at -46°C. This risk will be increased if you are using high heat input.

If you are using this type electrode, you are increasing the risk to have hydrogen cracks especially in the root. I would suggest to use GTAW or low hydrogen electrode (E7016-1) for the root pass.

 

Regards

 

F

 

 

 


Da: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Per conto di Jeremy Zibin
Inviato: martedì 29 settembre 2009 9.56
A: materials-welding@googlegroups.com
Oggetto: [MW:3361] Re: Heat Input

 

Gentlemen,


We've used qualified welding procedure specifications for LTCS that specifiy a root layer of 6010 (but only 1 root layer and no hot-pass) and then fill and cap layers with 7018.  This welding was performed on pressure piping under B31.3 for use in Northern Canada (min. design temp. of -46C).  The WPS was qualified, stamped by professional welding engineers and approved by the client.

It is my understanding that the root lay is limited in thickness on the WPS and therefore the total thickness and properties of the full weld are majority 7018, which is approved for LTCS.  The heat input is limited to a max. on the WPS so that the welded joint should have the adequate impact properties at low temperatures.  This will be proven during qualification but remember not to limit yourself on heat input on the WPS, use a typical heat input for your welding process and material thickness to pass the qualification.

 

Regards,

 

JZ

 


--- On Mon, 9/28/09, Muhammed Ibrahim <ibratech@gmail.com> wrote:


From: Muhammed Ibrahim <ibratech@gmail.com>
Subject: [MW:3358] Re: Heat Input
To: materials-welding@googlegroups.com
Received: Monday, September 28, 2009, 11:16 PM

E6010 will support up to -29 degree celcius only and used in pipe line root application. But if the PQR passes the impact you can use it with batch restriction.

regards,

Ibrahim

2009/9/29 BHARAT GOLE <bharatgole@hotmail.com>

E 7018-1 is acceptable up to -46 degree but selection E 6010 is not suitable for LTCS ! As per which clause it is selected for LTCS ?

Regards

Bharat B. Gole

 




Date: Tue, 29 Sep 2009 09:49:23 +0530
From: nach_sam@yahoo.com
Subject: [MW:3354] Re: Heat Input
To: materials-welding@googlegroups.com

Adi,

Heat input is a guideline for subsequent welding. The yardstick is the average  value as obtained from your PQR. Your production welding should not exceed PQR HI values.

By the way, is 6010, 7018-1 Ok for LTCS?  What is the working temp?

Shashank Vagal

--- On Tue, 29/9/09, Adi <adinraos@gmail.com> wrote:


From: Adi <adinraos@gmail.com>
Subject: [MW:3352] Heat Input
To: "Materials & Welding" <materials-welding@googlegroups.com>
Date: Tuesday, 29 September, 2009, 9:35 AM



I have done the PQR for LTCS by using 6010 & 7018-1 as per ASME SEC IX
some time i got 5KJ heat in put
What is the limitation for heat input and where it is mention?

Adi


From cricket scores to your friends. Try the Yahoo! India Homepage!</a

 


Get easy photo sharing with Windows LiveT Photos. Drag n' drop

 

 




--
Thanks & Regards
Muhammed Ibrahim PK

 


Be smarter than spam. See how smart SpamGuard is at giving junk email the boot with the All-new Yahoo! Mail </a

 

 

******************************************************************************************
CONFIDENTIALITY NOTICE
This e-mail and any attachment are confidential and may be privileged or otherwise protected from disclosure. It is solely intended for the person(s) named above. If you are not the intended recipient, any reading, use, disclosure, copying or distribution of all or parts of this e-mail or associated attachments is strictly prohibited. If you are not an intended recipient, please notify the sender immediately by replying to this message or by telephone and delete this e-mail and any attachments permanently from your system.

 


Make your browsing faster, safer, and easier with the new Internet Explorer® 8. Optimized for Yahoo! Get it Now for Free! </a


******************************************************************************************
CONFIDENTIALITY NOTICE
This e-mail and any attachment are confidential and may be privileged or otherwise protected from disclosure. It is solely intended for the person(s) named above. If you are not the intended recipient, any reading, use, disclosure, copying or distribution of all or parts of this e-mail or associated attachments is strictly prohibited. If you are not an intended recipient, please notify the sender immediately by replying to this message or by telephone and delete this e-mail and any attachments permanently from your system.



Looking for the perfect gift? Give the gift of Flickr!
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...