Skip to main content

[MW:3343] Re: ACCEPTANCE OF ROUNDED INDICATION BY VISUALL INSPECTION

Dear Asad,

The acceptance of PT can't be used for visual defect as this is the acceptance for size of indication only not the size of the defect. 4mm indication may come from 1mm pin hole. It depends on the amount of dye contained by the defect which comes out from the defect (due to blotting action) when developer applied.

The size of defect you are refering may give you 15-20mm indiacation.

Regards.
CK

2009/9/28 asad azmi <azmiasadayub@gmail.com>
GOODMORNING...........
 
can anybody can confirm  whether a pin hole of diameter 3mm and depth of approximately 5 mm in fillet weld  of 6mm of material SA 516GR 70  can be VISUALLY accepted. The vessel is fabricated as per ASME SEC VIII DIV 1.
 
If YES then by which code.
 
Kindly note that if we consider acceptance crieteria  for PT/MT, as per ASME SEC VIII DIV 1, APPENDIX 6/8, Rounded indication upto 4.8mm is acceptable.
 
can the above defect can be accepted on the basis of acceptance crieteria of PT/MT.
 
 
please reply ASAP.
 
Thanks & Regards
 
Asad Azmi



--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...