The Minimum Average Strengh for ER-70S-3 is -30°C at 27J. The Maximum is until it goes.
a hug,
Norberto de Souza Barbosa-Brazil
Subject: Re: [MW:4673] ER70S-3 for low temperature application
From: george.dilintas@gr.bureauveritas.com
Date: Fri, 2 Apr 2010 16:13:22 +0200
To: materials-welding@googlegroups.com
Then you will find your answer in USC-67.
If you do not have the code or you have interpretation problems let me know.
From: Muhammed Ibrahim [ibratech@gmail.com]
Sent: 02/04/2010 16:34 ZE4
To: materials-welding@googlegroups.com
Subject: Re: [MW:4670] ER70S-3 for low temperature application
--
Thanks & Regards
Muhammed Ibrahim PK
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Veja todos os seus e-mails de diferentes contas com apenas um login. Veja como.
a hug,
Norberto de Souza Barbosa-Brazil
Subject: Re: [MW:4673] ER70S-3 for low temperature application
From: george.dilintas@gr.bureauveritas.com
Date: Fri, 2 Apr 2010 16:13:22 +0200
To: materials-welding@googlegroups.com
Then you will find your answer in USC-67.
If you do not have the code or you have interpretation problems let me know.
From: Muhammed Ibrahim [ibratech@gmail.com]
Sent: 02/04/2010 16:34 ZE4
To: materials-welding@googlegroups.com
Subject: Re: [MW:4670] ER70S-3 for low temperature application
Hi,
The code is ASME SEC. VIII Div.1.
Regards,
Ibrahim
On 2 April 2010 09:58, <george.dilintas@gr.bureauveritas.com> wrote:
Could you clarify what is the application code? Section I, section VIII-1?
From: Muhammed Ibrahim [ibratech@gmail.com]
Sent: 01/04/2010 18:40 ZE4
Subject: [MW:4661] ER70S-3 for low temperature application
Hi members,Please provide a suggestion for the following query.I have qualified a PQR for GTAW+SMAW with ER70S-3 & E7018-1. The PQR is impact tested at - 46 deg C at root(GTAW) and filling (SMAW) and passed (Min. 50J energy obtained).As per ASME Sec.II part C, E7018-1 will support up to - 46 Deg C, but ER70S-3 will support up to - 20 Deg.C only.Since I have proven the toughness through PQR, can I use this PQR for job with impact test requirement of - 46 Deg C, even ER70S-3 does not support for this temperature as per Sec.IIC?.
Thanks & Regards
Muhammed Ibrahim PK
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
Thanks & Regards
Muhammed Ibrahim PK
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Veja todos os seus e-mails de diferentes contas com apenas um login. Veja como.
Comments