Skip to main content

Re: [MW:28320] For Demand Critical weld as per AWS D1.8

Consumable lot change need to do requalification  again . Even you can do test at Manufacturer end and get the 3.2 certification consumable MTC . 
Lincoln and ESAB is well aware of demand critical Weld qualification .other manufacturers also be contacted.
Sorry I can't share the copy of PQR and WPS which is approved by aramco.



P.NEILASHKUMAR 
Sent from my iPad
MOB :   +91 9952110791

On 22-Sep-2018, at 1:38 PM, Jibin Philip <jibinphilip123@gmail.com> wrote:

Neilash, 

Thank you so much  for you reply.So the conclusion is that we need to go for  ( two ) PQR - 3G & 1G position and make one WPS with both the values.Also the consumable batch used in PQR need to be followed in production weld. Am i correct??

Suppose our consumable lot change we need to go for new PQR or not ( as essential variable ).... Or any other option to tackle this??
If possible can u share ur PQR /WPS ( for reference only ) to my personnel mail : jibinphilip123@gmail.com

Regards, 
Jibin philip.

On Fri, Sep 21, 2018 at 10:01 AM 'Neilash Kumar' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Jibin ,

Normally demand critical welds , there is restriction in heat input , u need to consider and record high heat input welding using 3G vertical position and low heat input welding using 1G flat position ,both need to be addressed in PQR and WPS .
Also for demand critical Weld consumable lot is an essential variable , where the same lot to be used in production and WPS PQR . 
For this u need to take approval from Manufacturer and from your Management to proceed with TPI . 
Demand critical welds should be identified in drawing by engineering , so that u can proceed further .
Hope this clarifies , u can reach me below for further any clarification.
Recently I have done this qualification for aramco project .
P.NEILASHKUMAR 
Sent from my iPad
MOB :  +91 9952110791

On 21-Sep-2018, at 10:55 AM, CHITTARANJAN BHIWANDKAR <crbhiwandkar.smspl@gmail.com> wrote:

Mr. JIBIN PHILIP,
THIS S275JR IS A STRUCTURAL NON ALLOY STEEL EQUIVALENT OF IS2062.
HOW EVER IN ANY WELDING HEAT INPUT IS ALWAYS CONTROLED THROUGH WPS
BY WAY OF TRAVEL SPEED. THE FORMULA FOR HEAT INPUT IS (v*a) / travel speed.
ANOTHER FACTOR TO REDUCE THE HEAT IN PUT IS TO PREHEAT THE JOB.
Thanks/Regards,

C.R.Bhiwandkar
Supreme Megastructures Pvt. Ltd.
Supreme House, Plot No.-49/C,
Pratap Gad, Opp.-IIT Main Gate.
Powai, Mumbai - 400076
Cell No.:-+919867139337



On Thu, Sep 20, 2018 at 3:33 PM Jibin Philip <jibinphilip123@gmail.com> wrote:
Dear All, 

PQR : Code : AWS D1.1
Welding Process - FCAW ( E71T-1C )
Filler Size - 1.2mm
Material - S275JR to S275JR

For Demand Critical weld as per AWS D1.8, is there any heat Input restrictions are to be followed or not??. In our current WPS the Heat input mentioned are 0.6 to 1 kj/mm.Is this acceptable for Demand Critical weld application ??.  In AWS D1.8 - clause 6.8.1 mentioned as " The heat input range qualified by testing in accordance with Annex A. In annex A it showing a range of 1.2 to 3.1 kj/mm. Dear Experts please help .

Regards, 
Jibin philip

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...