[MW:28289] Re: Can I use WPS/PQR P NO-1, Group NO-1 (PLATE) to P NO-1, Group NO-2 (PLATE) for welding of ASTM A333 Gr.6 (P No: 1, Group No: 1) to ASTM A350 Gr.LF2 CL.1 (P No: 1, Group No: 2) ?

Lets consider your case, the contractor is having Pipe (P1G1), Flange/ Fitting (P1G2). and may be going to have joints between

1. P1G1 to P1G1 (pipes to pipe)
2. P1G1 to P1G2 (pipe to fitting)

with above consideration,the qualification mandate CVN variable so the contractor require to have qualified WPS as per ASME Section IX for P1G1 to P1G1 and P1G1 to P1G2.
you must check the range of material thickness involved (You may need a combination of PQR/WPS to cover the thickness range for each above grouping).  Refer AW 403.5 & QW 403.6 for detailed condition.

Thanks & regards
Sandeep Kumar


On Friday, August 24, 2018 at 4:58:41 PM UTC+3, Chiranjeevulu Temburu wrote:
Dear Experts,

1. WPS/PQR (P NO: 1, Group No-1 to P NO: 1, Group No-1 ) is available with contractor

2. Pipe material: ASTM A333 Gr.6 (P No: 1, Group No: 1)

     Flange/Fitting material: ASTM A350 Gr.LF2 CL.1 (P No: 1, Group No: 2)

     WPS/PQR ( P NO: 1, Group No-1 to P NO: 1, Group No-2 ) is not available with contractor 

3.  Charpy "V" notch test to be done

My query is 
 
Can I use WPS/PQR P NO-1, Group  NO-1 (PLATE) to P NO-1, Group NO-2 (PLATE)   for welding of  ASTM A333 Gr.6 (P No: 1, Group No: 1) to ASTM A350 Gr.LF2 CL.1 (P No: 1, Group No: 2) ?

Please give suggestions, Is it possible in accordance with ASME Section-IX  ?



CHIRANJEEVULU TEMBURU l Inspection Engineer-Mechanical I +918790956353.



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...