Re: [MW:21251] RE: 21247] peening as a temporary repair

If defect is known, it should be removed completely prior to repair. Superficial repair would be is not a solution. Even if you apply NBIC code (since it is in service), defect has to be removed prior to repair.
 


On Wed, Jun 25, 2014 at 7:04 AM, 'nishant852003@yahoo.com' via Materials & Welding <materials-welding@googlegroups.com> wrote:

Dear all,
Greetings from my side,

I too agree to the fact that Mr. Bapat has mentioned. Peening the weld in steam service has higher risk level especially pressure vessel. In case of low pressure steam service try to arrest the leak with the help of online sealing as a temporary measure, provided its an emergency. Later on as mentioned by Mr. Bapat, go for complete UT and find the leak path.

Sent from Yahoo Mail on Android



From: Ramesh Bapat <rbapat@hotmail.com>;
To: <materials-welding@googlegroups.com>;
Subject: [MW:21248] RE: 21247] peening as a temporary repair
Sent: Wed, Jun 25, 2014 2:05:14 AM

I suggest against it in an existing vessel in steam service.  Peening may take care of a surface indication or stop up a pin hole leakage, but  one has no idea if the root cause may or may not be a lot bigger than what can visually be detected.  Steam is erosive. It will eat metal away fast.   Also if steam flashes, it can hammer, which will result in the possibility of high stress concentrations at points of stress risers in such as nozzle to shell welds (corner joints) which over time, can cause stress cracking.  I suggest you to take this vessel out of service, perform a UT examination at the location of the indication (Try to discover the path of failure), remove the defective weld to sound metal by grinding, PT examine the repair area, re-weld it, PT the cover pass, perform local PWHT if required by code, and re-hydro test it.  I would not risk the possibility of blowing a nozzle off the vessel wall for a quick fix of a leaky weld in steam service. Thanks

 

Ramesh Bapat

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Adriaan Stoltz
Sent: Tuesday, June 24, 2014 6:05 AM
To: materials-welding@googlegroups.com
Subject: [MW:21247] peening as a temporary repair

 

Good day valued members.

 

Has any of you gentlemen had any experience in temporary repairs on carbon steel pressure vessel by means of mechanical peening? A steam leak was discovered on a Low pressure Heater (300Kpa) at a nozzle to vessel shell weld interface. It seems to be a pinhole through the weld. Is mechanical peening of the defect area considered to be an acceptable means of closing up the leak temporarily until a proper weld repair can be carried out?  And if so, is this type of repair documented in any of the in service inspection and repair standards?

Your input is greatly appreciated.

 

 

Riaan Stoltz

RITC Inspection

083 6405909

021 556 4884

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...