Skip to main content

Re: [MW:21290] QW-452.3 GROOVE-WELD DIAMETER LIMITS

Dear Rajesh,

Hope this will help.

The following interpretation of ASME Section IX applies to Set-through and Set-on nozzle installation:
Interpretation: IX-80-67
Subject: Section IX, Nozzle to Shell Connections
Date Issued: December 8, 1980
File: BC-80-675
Question: When nozzle or branch connections are attached to the wall or head of a pressure vessel, what are the basic criteria establishing procedure and performance qualification requirements, assuming impact test is not a requirement?

Reply: Where the nozzle is attached to the vessel by welding completely through the thickness of the vessel wall, the procedure shall be qualified for the thickness of the vessel wall penetrated by the nozzle or attachment. Where additional metal is placed on either the interior or exterior of the vessel wall in the form of fillet welds, they shall be considered as having been qualified by the procedure qualification covering the thickness of the vessel wall. Performance qualification for this weldment may be made in plate to cover the appropriate thickness of the vessel wall and the position in which the weld is being made. Diameter is not a factor.

Where the nozzle or attachment is welded to the vessel wall by welding through the thickness of the nozzle or attachment, the procedure qualification shall be made for the thickness of the nozzle or attachment wall at the time of welding. Performance qualification for this condition shall be made with the appropriate diameter pipe as required by QW-452.3, with the range of thickness of weld metal qualified determined by the thickness of the nozzle or attachment wall at the time of welding. Any fillet welds, both procedure and performance, will have been qualified when qualifying for the full penetration welds involved.

Note: The above interpretation refers to nozzle attachment to vessels, however the criteria apply to branch attachments topressure piping as well.

--------------------------------------------
On Sat, 6/28/14, rajesh s. mhaske ,Engineer Welding ,PUNE,INDIA <rajesh.mhaske17@gmail.com> wrote:

Subject: Re: [MW:21289] QW-452.3 GROOVE-WELD DIAMETER LIMITS
To: materials-welding@googlegroups.com
Date: Saturday, June 28, 2014, 12:50 PM

   Dear sir
              
Any reference document for below statement/ case study/Asme
interpatation copy . I have to give it to third party
inspector.
Now we are doing same but don't have document for
reference

On Saturday, June 28, 2014 11:45:12 AM UTC+5:30, veera
raghava kommisetti wrote:Set-on Type -
Not qualified.Set-In Type -
Qualified.

On Fri, Jun 27, 2014 at
11:35 AM, rajesh s. mhaske ,Engineer Welding ,PUNE,INDIA
<rajesh....@gmail.com> wrote:


Dear sir
          
Pipe dia : 323.*33 mm thk
          
Tube dia : 50.8 *6.35 mm thk
          
Groove design for  above pipe to tube welding  :
set in (groove on header )  / set on (groove on
tube  )

          
Welding process : GTAW + FCAW

          
Qualification of welder: OD >73 mm and Thk - Max to be
welded with process GTAW+FCAW
          

Question :
           
1) Can above qualified welder be deployed for welding of set
in and set on joint.

           





--

To post to this group, send email to material...@ googlegroups.com

To unsubscribe from this group, send email to materials-weld...@ googlegroups.com

For more options, visit this group's bolg at http://materials-welding.
blogspot.com/

http://www.linkedin.com/
groups/MaterialsWelding-
122787?home=&gid=122787&trk= anet_ug_hm


 

The views expressed/exchnaged in this group are members
personel views and meant for educational purposes only,
Users must take their own decisions w.r.t. applicable
code/standard/contract documents.

---

You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails
from it, send an email to materials-weld...@ googlegroups.com.

For more options, visit https://groups.google.com/d/
optout.







--

To post to this group, send email to
materials-welding@googlegroups.com

To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

 

The views expressed/exchnaged in this group are members
personel views and meant for educational purposes only,
Users must take their own decisions w.r.t. applicable
code/standard/contract documents.

---

You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails
from it, send an email to materials-welding+unsubscribe@googlegroups.com.

For more options, visit https://groups.google.com/d/optout.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...