First You have to select the suitable Electrode/Filler Rod from your experience or based on Technical Literature.
 
The suitable electrode for welding IS2062 Gr.A to SS 410 is either E309L or Nickel based consumables like ENiCrMo3/E NiCrFe2/3.
 
Then check for the A.No in QW-442 as A8 for E309L & A4X for Nickel based electrodes
 
Then based on the SFA number(obtained from Sec.IIC) for the particular electrode, F number can be determined like F5 for E309L etc...

J.GERALD JAYAKUMAR
00919344954677
 


--- On Tue, 2/22/11, puneet takiar <puneet1takiar@yahoo.com> wrote:

From: puneet takiar <puneet1takiar@yahoo.com>
Subject: Re: [MW:9967] P1 no Range
To: materials-welding@googlegroups.com
Date: Tuesday, February 22, 2011, 5:42 AM

Dear Colleagues,
Can anybody help me in describing method to select Electrode for welding SS to M.S ( IS2062 Gr.A to SS 410).
As per sextion IX table QW 442, A no. will be 6 ( is it ok) and how i can find F no. w.r.t A no. whether there is any coorelation of A no. with F no. or not? OR their function is different w.r.to each other. please help.
 
If  the F no. is to be selected by experience then how the table of F no. in QW 432 is helpful.
 
Warm regards, 
puneet takiar



From: jaya anil <nethalaanil@gmail.com>
To: materials-welding@googlegroups.com
Sent: Mon, 31 January, 2011 6:18:40 PM
Subject: Re: [MW:9601] P1 no Range

Dear Puneet,
 
IS 2062 Gr A, is unlisted , but max. properties were equalent to P1. but while preparing WPS/PQR use Material Spec as IS 2062 GrA .
 
SS 410 is Martensitic Steels, its P No is 6

On Sun, Jan 30, 2011 at 8:04 PM, puneet takiar <puneet1takiar@yahoo.com> wrote:
Hello!
Can anybody tell me in which P. no IS 2062 grade A and SS 410 will fall and how to search in ASME sex IX table.
Regards, 
puneet takiar



From: Karthik <karthik6684@yahoo.com>
To: materials-welding@googlegroups.com
Sent: Fri, 7 January, 2011 1:46:08 PM
Subject: Re: [MW:0] P1 no Range

Hi,
Please refer QW423 also QW 350 for essential variables.

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Fri, 1/7/11, sn vl <weldinspn@gmail.com> wrote:

From: sn vl <weldinspn@gmail.com>
Subject: [MW:9122] P1 no Range
To: "Materials & Welding" <materials-welding@googlegroups.com>
Date: Friday, January 7, 2011, 2:43 PM

Hi..

How to find in ASME sec IX P no to Pno qualification range.
Eg : If a welder qualified for P1to P1
what is the Range qualified As per Sec IX.
Where is given in CODE.


Regards
SN.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...