Skip to main content

[MW:2974] Re: Alloy Steel

You have to weld in a ' stitching progression '  from the cente outwards so that the heat input is distributed evenly and slowly,
 
you need to weld 50 - 100 mm then stop then move 100 mm and weld another 100 mm, from the centre outwards,
 
you then return to where you started and complete the rest of the un welded areas
 
this will prevent the shrinkage,
 
Nick Davies

On Wed, Aug 19, 2009 at 3:25 PM, Mrityunjay Kumar / ZS Saudi PEB QA/QC <Mrityunjaykumar@zamilsteel.com> wrote:

Dear all,

 

We have encountered that the material (8 mm plates from ASTM 572 Gr-50, Type-1) is shrinking along to the length while doing double side welding at flange of the crane beam.

Anyone can explain the reasons of above problem.

 

 Thanks and Regards,

M.K.Choudhary

     

      PEB - QA/QC

P.O. Box 877, Dammam 31421

Kingdom of Saudi Arabia

'   +966 38471840 Ext- 555

7    +966 38471840 Ext-559

ý   www.zamilsteel.com

 

 


--------------------------------------------------------------------------------------------------------
Disclaimer: This email and any files transmitted with it are confidential
and intended solely for the use of the addressee(s) named herein. If you
are not the intended recipient or addressee, you should not use, disseminate,
distribute, copy or alter this email. Any views or opinions presented in this
email are solely those of the author and might not represent those of "Zamil
Industrial" and or its units.

Warning: Although reasonable precautions have been taken to ensure no viruses
are present in this email, the company cannot accept responsibility for any
loss or damage arising from the use of this email or attachments. If you have
received this electronic mail message in error, please contact the sender directly.



--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...