Skip to main content

Re: [MW:22422] G type consumable

BEGIN:VCARD
X-LOTUS-CHARSET:UTF-8
VERSION:3.0
PRODID:-//Lotus Development Corporation//NONSGML Notes 8.5.2//EN_C
FN:George H Dilintas/GRC/VERITAS
N:Dilintas;George;;;
ADR;TYPE=WORK;TYPE=PREF:PIRAEUS;;23\, Etolikoy Str.;PIRAEUS;;185 45
;GREECE
ADR;TYPE=HOME;TYPE=PREF:;;19-21 B. Laskou str.;Athens;Attika;11 633
;Greece
TEL;TYPE=HOME:+30-1-7667 197
TEL;TYPE=WORK:+30-210-40 63 113
TEL;TYPE=HOME;TYPE=FAX:+30 - 1 - 7667 197
TEL;TYPE=WORK;TYPE=FAX:+30-210-40 63 118
TEL;TYPE=CELL:+30 -69 44-64 62 04
EMAIL;TYPE=WORK;TYPE=PREF;TYPE=INTERNET
:george.dilintas@gr.bureauveritas.com
ORG:Bureau Veritas;Industry
REV:20131201T024559Z
END:VCARD

The A-number is not assigned. It is determined on the basis of the actual chemical composition of the weld metal.
For certain processes (GMAW, SAW, ....) a chemical analysis of the weld metal is required.

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor


    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    (See attached file: Dilintas_George.vcf)

John Henning ---28/11/2014 19:16:59---A -G consumable does not meet any particular ASME/AWS SFA/A-5.x classification chemistry.  This does

From: John Henning <jhenning@deltak.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Date: 28/11/2014 19:16
Subject: Re: [MW:22400] G type consumable
Sent by: materials-welding@googlegroups.com




A -G consumable does not meet any particular ASME/AWS SFA/A-5.x classification chemistry.  This does not mean that it will not meet a Section IX A-Number chemistry range.  You would need to evaluate the filler metal manufacturer's specified chemistry range to see if it fits one of the A-number chemistry ranges.  Alternatively, you can specificy that the filler metal must meet a certain range.  While not a G filler metal, I typically specify that ER70S-6 must meet the A-Number 1 chemistry requirements.



From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> on behalf of Pravin Poornachandran <htcispravin@gmail.com>
Sent:
 Friday, November 28, 2014 5:58 AM
To:
 materials-welding@googlegroups.com
Subject:
 [MW:22396] G type consumable 
 
Dear expert,
Is it true that all G type consumable example ER70S-G don't have A number under ASME?
This group only have F number? Is it true?
Kindly advice.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...