Dear Mohit,
 
Although your query lack all necessary information like the applicable code, the type of consumable, materials etc but on a general note, welders qualified for clad restoration are not qualified to weld butt joints but when a welder is qualified on butt weld, the weld is qualified to weld clad restoration if only
 
1. requirement for Chemical composition.
 
2. within the F number of the consumable qualified,
 
3. within the welding position qualified
 
Please refer to ASME IX Art III (See Below)
 

QW-381.3 Alternative Qualification With Groove

Weld Tests.

When a chemical composition is not specified

in the WPS, welders or welding operators who successfully

complete a groove weld performance qualification

test meeting the corrosion

resistant overlay bend test requirements

of

QW-163 may be considered qualified for

corrosion

resistant overlay welding within the ranges defined

in

QW-350 or QW-360.
Regards,
 
Rems Okonkwo
IWE Nigeria
On Thu, Sep 25, 2014 at 3:43 PM, Mohit Aggarwal <aggarwalmohit05@gmail.com> wrote:

Dear Experts,

I have query regarding welder that if a welder is qualified for clad restoration overlay then he will be qualified to weld in groove joint or not.

If a welder is qualified for groove welding,then he will be qualified for clad restoration overlay or not.

Thanks!!

Best Regards,
Mohit Aggarwal.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...