Tuesday, September 23, 2014

Re: [MW:21972] Lack of fusion in production welding - GMAW !!!

short circuit  is not suitable for thickness more than 13mm

THANKS & BEST REGARDS
KG.PANDITHAN, AWS-CWI, CSWIP 3.1
CONSULTANT-WELDING & QUALITY

On Mon, Sep 22, 2014 at 5:57 PM, Vadivel Mahadevan <vadivelmahadev@gmail.com> wrote:
Hello Mr. George,
My LOF is intermittent in majority of the jobs. However in fewer bodies it is continous. I can say 85:15 ratio of the Leaked welds
Regards
Vadivel. M

On Saturday, September 20, 2014 4:10:26 PM UTC+5:30, George Dilintas wrote:

Your LOF is intermittent of continuous?
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: Vadivel Mahadevan [vadivel...@gmail.com]
  Sent: 09/20/2014 02:19 AM MST
  To: material...@googlegroups.com
  Subject: [MW:21945] Lack of fusion in production welding - GMAW !!!


Dear Experts,
 
I face Lack of fusion problem in GMAW process in the production weld often.
WPS qualified on short circuiting mode as the torch is designed to the same.
But when I use the same current and voltage I come across Lack of fusion
The wire I use is ER316L of 1.2mm dia.Bare wire , volt not more than 19V.
 
Now I started using 23 to 26V(Spray transfer mode volt range) to overcome my issue.
Can you suggest what are the parameters I need to control to get a sound weld in the short circuiting mode.
 
Regards
Vadivel. M
07829007400

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...