Sunday, September 21, 2014

Re: [MW:21964] ASTM A 316L Material PWHTed

Chck microstructure for presence of any grain boundry carbide precipitations. 

IGC test accrding to E262 canbe done.



On Sunday, September 21, 2014, Ramin Kondori <raminkondori@gmail.com> wrote:
The safest solution is to cut & remove the joint (cut length shall be equal to or longer than minimum pipe length as in specification) and replace the pipe...

But if you have to keep it, you should know the operation requirements (fluid, temp, corrosion parameters etc.)...
Usually if it is S-316L (low carbon grades will not degrade drastically if stress relieved) and corrosion is not severe, you can proceed but leave a note for RBI team to keep an eye on it and examine it periodically.
  

Best Regards

Ramin Kondori

Sr. QA/QC engineer

Yadavaran Oilfield Project

SIPC (SINOPEC)


On Sat, Sep 20, 2014 at 4:09 PM, Arumugam Dinesh Kumar <adineshk68@rediffmail.com> wrote:

Dear friend ,

Carry out in-situ metallograpy on the joint to understand the occurence of sensitization . Generally
in-situ metallography facilities are remotely available . Instead carry out 6in length weld of same thk
and subject to same parameters of PWHT and examine for sensitization.

Regards
Dinesh

On Sat, 20 Sep 2014 16:08:22 +0530 Amul Raj wrote
>Dear Experts,

In our Shaybah project (Saudi Aramco) 28 mm Thk 316L material weld joint by mistakenly done PWHT

So what is the solution for this, is it acceptable

What is the further action, how we conform theweld material there is no any changes in mechanical &
chemical properties


Regards,

Amul Raj Thanga Velu

QA/QC Welding

Samsung Engineering



--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>
For more options, visit this group';s bolg at http://materials-welding.blogspot.com/
>
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>

>
The views expressed/exchnaged in this group are members personel views and meant for educational
purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
---
>
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
>
To unsubscribe from this group and stop receiving emails from it, send an email to materials-
welding+unsubscribe@googlegroups.com.
>
For more options, visit https://groups.google.com/d/optout.
>

Get your own FREE website, FREE domain & FREE mobile app with Company email.  
Know More >

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...