Re: [MW:17239] WPS with PWHT below the lower transformation temperature

As Mr Pal written, temp is restricted as per 31.3
Pandithan
welding consultant

On 3/27/13, Biplab Pal <biplab.mech@googlemail.com> wrote:
> Dear Mohd.,
>
> As per ASME B-31.3 Table 331.1.1 you have to do PWHT within the specified
> range of 593 deg C to 649 deg C (for P-No-1) you can not do or write beyond
> that limits.
>
>
>
> On Sat, Mar 23, 2013 at 10:20 AM, mohd <mohd52100@gmail.com> wrote:
>
>>
>> Dear all,
>>
>> WPS details as per ASME IX Design Code :B31.3
>>
>> 1) GTAW + SMAW (3mm+ 24mm)
>> 2) Material API 5L x52 Thk : 26.97
>> 3) PWHT 600 +/-20 Time : 1Hr 20min
>> 4) No impact.
>>
>> Can I Re Write WPS with Temperature 670+/-20 as per As per QW-407.1 a
>> (2)
>> ? ( up to below Lower transformation no need re qualification )
>>
>> Need expert Opinion.
>>
>> ( QW-407 Postweld Heat Treatment
>> QW-407.1 A separate procedure qualification is
>> required for each of the following:
>> (a) For P-Numbers 1 through 6 and 9 through 15F materials,
>> the following postweld heat treatment conditions
>> apply:
>> (1) no PWHT
>> (2) PWHT below the lower transformation temperature )
>>
>>
>>
>> Regards,
>> mohd.
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>>
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views
>> and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>> ---
>> You received this message because you are subscribed to the Google Groups
>> "Materials & Welding" group.
>> To unsubscribe from this group and stop receiving emails from it, send an
>> email to materials-welding+unsubscribe@googlegroups.com.
>> For more options, visit https://groups.google.com/groups/opt_out.
>>
>>
>>
>
>
>
> --
> Thanks & Regards
> Biplab Pal
> Welding Inspector
> E-mail: biplab.mech@gmail.com
>
> Information in this email and any attachments is confidential and intended
> solely for the use of the individual(s) to whom it is addressed or
> otherwise directed. Please note that any views or opinions presented in
> this email are solely those of the author and do not necessarily represent
> those of the Company. Finally, the recipient should check this email and
> any attachments for the presence of viruses. Myself accepts no liability
> for any damage caused by any virus transmitted by this email.
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...