Re: [MW:13784] RE: 13168] Low Hydrogen Electrode in Steel Structure Application

Dear all,
 
         I would like to add small comments addition to Mr Kaja, Baking and holding is not required if the electodes used directly from vacuum packed carton which is manufacturer package.
 
regards
IK

On 8 December 2011 14:03, Kaja Mohideen <kaja@asw.sa> wrote:

Dear Mr. Endri,

 

All kinds of basic coated Electrode (Low Hydrogen) must be baked for (E7018) at 230 degrees for 2hours then it transferred to Holding oven at 120 degrees for continuous use, After that you can issue the electrode from holding oven to portable oven at Minimum 60 degrees maintain for shop and Site welding,  Electrode return to holding oven at the end of the shift which electrode not exposed to atmospheric for the Maximum hours, So when the electrode exposed above the maximum hours, it shall be rebaked once, the rebaked electrode shall not be rebaked again, should scrap.

 

It's all about to prevent the electrode to control Moisture Pickup

 

Refer AWS A5.1: Specification for Carbon steel Electrode

 

Best Regards,

Kaja Mohideen

QA/QC Manager

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Endri Prasetyo
Sent: Thursday, December 08, 2011 11:55 AM
To: materials-welding@googlegroups.com
Subject: [MW:13168] Low Hydrogen Electrode in Steel Structure Application

 

Dear Experts,

Anybody can advice please, when we use low hydrogen type electrode for steel structure welding erection (SMAW process) does it require to be baked all the time @70 C deg on work station?
Is it acceptable when the welder only keep the electrode into the portable oven without baking (after issued from holding oven) although it is a not best practice?
For information, the material of the steel structure is carbon steel Q235.

Appreciate your sharing. Thanks.

Regards,
Endri

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...