RE: [MW:13767] Incomplete pen vide B31.3 2004 Ed

Hi

 

Ref B31.3

 

The applicable NDT method for this defect is VT and RT.  If it is an open joint check the depth of IP by visual. But in RT you can approximately identify( Not measure) the depth by difference in contrast relative to the IQI contrast at that location

BR

M.Vijayan

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Shashank Vagal
Sent: Tuesday, February 21, 2012 2:12 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:13764] Incomplete pen vide B31.3 2004 Ed

 

Thanks, Manpreet and others,
It was captured during RTFI and the lengths were 12 mm and 25 mm at 2 different locations. I have already given both as repair. But the contractor came with this table which shows Category M fluid, girth weld, weld imperfection ' Incomplete Pen' is referred to as B. On the following page, B refers to "depth" of IP to between ≤1mm and ≤ 0.2Tw (whichever is lower is implied) and not length. Now, that is one tough task to determine depth of an IP, by RT at least. In Cum Length, < 38 mm in 150 mm, we have acceptance.
So, is my judgement correct or no?
Best regards,
Shashank Vagal


--- On Tue, 21/2/12, manpreet <manpreetsin88@rediffmail.com> wrote:


From: manpreet <manpreetsin88@rediffmail.com>
Subject: Re: [MW:13762] Incomplete pen vide B31.3 2004 Ed
To: materials-welding@googlegroups.com
Date: Tuesday, 21 February, 2012, 1:49 PM

Hi,

As per ASME B31.3, acceptance criteria for incomplete penetration is:- between ≤1mm ann ≤0.2Tw

was it caught by Radiography or ultrasonic testing?

If UT then there is possibility that what you are referring to "incomplete penetration" might
actually be "Lack of sidewall fusion" for which table 341.3.2 Note 7 states that
"tightly butted unfused root faces are unacceptable".

Regards
Manpreet Singh



On Tue, 21 Feb 2012 09:11:51 +0530 wrote
>Gents,
REF:
B31.3 Ed 2010, Table 341.3.2
Weld joint of 8" dia x 7 mm thick 106 Gr B, Fluid Service Normal, Category M.
Welding Process: GTAW + SMAW.
Is incomplete pen allowed as per this code to any extent ? Please advise.
Regards,
Shashank Vagal






--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for
educational purposes only, Users must take their own decisions w.r.t. applicable
code/standard/contract documents.
>

 

Follow Rediff Deal ho jaye! to get exciting offers in your city everyday.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



This communication and any files transmitted with it are confidential and may also be privileged. It is for the exclusive use of the intended recipient(s). If you are not the intended recipient or the person responsible for delivering it to the intended recipient(s), please note that any form of distribution, copying or use of this communication or information contained in it is strictly prohibited and may be unlawful. If you have received this communication in error please return it to the sender, and delete the material from any computer. We reserve the right to monitor email communications through normal internal and external networks. We believe but not warrant that the email and the attachments are virus free. The statement and opinions expressed in this communication are those of the writer and do not necessarily represent those of Madina Group, whose registered office address is

P.O. Box 20459, Doha, Qatar.
Tel. +974 44600818
Fax. +974 44603143

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...