Dear Kisan

As per QW404.22, addition or deletion of consumable inserts is non-essential variable for Welding Procedure Qualifications. You can use the same WPS.

However for Welding Performance Qualification, as per table Qw-356, addition or deletion of consumable inserts is "essential" variable for manual and semiautomatic GTAW. Thus your welder needs to be requalified with the consumable inserts.

Regards

Prem Nautiyal


On Mon, 17 Jan 2011 13:59:35 +0530 wrote
>
Hi Kisan,

As per ASME SEC IX QW 404.22 it is non essential
variable. So you can use as it with insert.
Please read below given Clause.
If any doubt is in your mind feel free to call or mail
me.



QW-404.22 The omission
or addition of consumable
inserts. Qualification in a
single-welded butt joint, with or
without consumable inserts, qualifies
for fillet welds and
single-welded butt joints with backing
or double-welded
butt joints. Consumable inserts that
conform to SFA-5.30,
except that the chemical analysis of
the insert conforms to
an analysis for any bare wire given in
any SFA specification
or AWS Classification, shall be
considered as having the
same F-Number as that bare wire as given in table
QW-432.
Thanks
& have a nice day
--
>With Warm Regards,
>Prakash Verma
>Metallurgist
-Drilling Riser Systems(Welding)
>QS Supply Chain.
>Aker Solutions Supply chain
hub-India
>AkerSolutions
>Tel.+91-20-66 28
8538,09503021486
>Email.
prakash.verma@akersolutions.com
>

>


From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Kisan
Gamane
>Sent: Monday, January 17, 2011 11:22 AM
>To:
materials-welding@googlegroups.com
>Subject: [MW:9254] WPS without
consumable insert
>
>

Dear Expert
Please advice me about following.

If WPS ( GTAW) is qualified for without consumable insert
; can we use it for with insert.
Code used for acceptance:- ASME sec IX

Thanks in advance for ur help.

Thanks & regards
>--
>


किसन
गामणे
नाशिक
After
falling twice to conquer the mount
Everest,
Edmund Hillary said-
>I'll come again and conquer you because as a mountain
you can't grow,
>but as a human I can..."
>
--
>To post to this group, send email to
materials-welding@googlegroups.com
>To unsubscribe from this group, send email
to materials-welding+unsubscribe@googlegroups.com
>For more options, visit
this group's bolg at http://materials-welding.blogspot.com/
>The
views expressed/exchnaged in this group are members personel views and meant for
educational purposes only, Users must take their own decisions w.r.t. applicable
code/standard/contract documents.
> This e-mail and any attachment are confidential and may be privileged or otherwise protected from disclosure. It is solely intended for the person(s) named above. If you are not the intended recipient, any reading, use, disclosure, copying or distribution of all or parts of this e-mail or associated attachments is strictly prohibited. If you are not an intended recipient, please notify the sender immediately by replying to this message or by telephone and delete this e-mail and any attachments permanently from your system.




--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>


PREM S NAUTIYAL
CELL : 9769316004

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...