Tuesday, October 26, 2010

Re: [MW:7815] SG Iron Welding

Hi

S.G Cast iron is defined as a high carbon containing, iron based alloy in which the graphite is present in compact, spherical shapes rather than in the shape of flakes, the latter being typical of gray cast iron .
Spheroidal graphite cast iron, are sometimes referred to as ductile iron OR Nodular iron also.

You can use the following M&R electrode for welding S.G Iron:

1) L&T Eutectic make - XUPER 2240
It is a ferro-nickel electrode and similar to ENiFeCI specs.
Polarity: AC/DC -
It has excellent machinability.
Complicated parts may require preheat upto 300 degree C.
Use short arc, peening, stringer beads and slow/retarded cooling.

Regards

Prem S Nautiyal
QA/QC & Welding Manager
Thermax Ltd., Pune
Cell: 9769316004

On Mon, 25 Oct 2010 18:23:07 +0530 wrote
>
Hi
All,
Can any body Suggest
me the welding of S.G.Iron (EN-JS 1025 / ASTM A 395) ?
Pl mention the
standard,Filler Materila details& procedure.

Regards,
Kiran
Panshetty,



******************************************

" Call 92256 37451 - Your helpline for everything in Steam "

DISCLAIMER:This e-mail message is proprietary to Forbes Marshall and is intended solely for the use of the entity to whom it is addressed. It may

contain privileged or confidential information exempt from disclosure as per applicable law. If you are not the intended recipient or

responsible for delivery to the intended recipient,you may not copy,deliver, distribute or print this message. If the contents are unrelated to

the Company's normal business activity it may be treated as personal views of the sender. The message and its contents have been virus checked.

but the recipients may conduct their own. FM will not accept any claims for damages arising out of viruses.

*******************************************





--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>


PREM S NAUTIYAL
CELL : 9769316004

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...