You can use ER70S-2 without requalification, since you are using a classification which exhibits greater toughness or recommended for lower temperature than the one used during procedure qualification.
QW 404.12 (e) applicable in your case.
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Muhammed Ibrahim
Sent: Thursday, May 13, 2010 9:09 PM
To: materials-welding@googlegroups.com
Subject: [MW:5165] Change in welding consumable when impact is required
Dear Members,
Please provide a clarification on the following query.
One PQR is qualified with GTAW+SMAW, ER 70S-3+E7018-1 and impact tested at-46.
Impact testing is required for the job at -29 Deg.C. Can I use ER70S-2 instead of ER70S-3 ?.
As per ASME Sec.II C, ER 70S-3 supports up to -20 Deg C & ER 70S-2 Supports up to -30 Deg.C.
Is QW 404.12 applicable in this change?.
Thanks & Regards
Muhammed Ibrahim PK
No comments:
Post a Comment