Dear Suresh,
Grind the surface just before the deposition and try. This might be due to Chromium oxide which has already formed on the surface. Also slow cool by wrapping the entire job with an asbestos cloth.

Srinivasan  


On Fri, Nov 20, 2020 at 9:37 PM SURESH <qms.pjgpl@gmail.com> wrote:
Dear sir
While welding itself I am getting crack.

Ring is holded in the positioner by means of clamps at 90 degree and we are proceeding the welding.


Regards
Suresh

On Friday, 20 November 2020 at 16:47:34 UTC+5:30 JS wrote:
Dear Suresh

Are you getting the crack during the deposition? Or after the job is cooled?

Srinivasan

On Fri, Nov 20, 2020 at 3:16 PM SURESH <qms....@gmail.com> wrote:
Dear Experts
During welding of Duplex grade material we are facing crack on the weld metal as attached in the photo. Below is the detailed process for reference

Process: PTAW
Base Material: ASTM 182 Gr.F55
Consumable: Stellite 12 (Powder)
PreHeat: Nil
Interpass: <200*C
Current: 128 to 145
Gas: Ultra Pure ARGON
Job Size: OD544 X ID 472 X Thk 36mm
Welding: Overlay weld on OD Surface alone


We are welding deposition thickness of 3mm. So as per this we are doing welding of 2 layer with multi pass, On welding second layer we found crack. Can anyone suggest where it is went wrong and why this crack is propagated. Please advice

 

In First layer- Total of 12 weld pass

In second layer- Total of 12 weld pass



Regards

Suresh

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8fd110ad-c422-4025-bf91-632d75b53a60n%40googlegroups.com.


--
J.SRINIVASAN
Mobile : 75501 82117



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b098ade0-08fa-49b1-8e31-afd4ad84e81an%40googlegroups.com.


--
J.SRINIVASAN
Mobile : 75501 82117



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKHQPVwPwqLG-p9X9Os89%3Dq7_pZ_AfauF4fEtVTj72J2GdpS5A%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...