Wednesday, March 6, 2019

Re: [MW:29202] RE: 28982] Backing gas as per API RP 582

if the root pass from the external surface, the slag should not provide any protection and it comes up to the surface. If no purging (with SMAW) I think the root would need reworking

Στις Δευ, 28 Ιαν 2019 στις 7:53 π.μ., ο/η PGoswami <pgoswami@quickclic.net> έγραψε:

Manoj,

 

SMAW never requires back purging. It's the "slag" generated by the process, which protects the weld root. This is just back to basic scenario.

Thanks.

 

P.Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Specialist

Saudi Aramco: Designated Project Welding Engineer(DPWR)& Quality Management Personnel

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@quickclic.net,pradip.goswami@gmail.com

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Manoj John
Sent: January 27, 2019 8:04 PM
To: materials-welding@googlegroups.com
Subject: [MW:28982] Backing gas as per API RP 582

 

Dear Experts,

 

As per clause 7.3 of API RP 582 Ed. 2016 back purging required for GTAW & GMAW process but no where I could found for other process like SMAW.  Is it mean that if we do welding with SMAW process back purging is not required?

 

Please share your interpretation.

 

Thanks and regards

 

Manoj.

 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...