Skip to main content

Re: [MW:27828] AWS D 1.1 interpretation on Increase in Preheat / Interpass temperature

Why don't get interpretation from aws which will be very useful for all members. Why this code is different in somany aspects on essential variable from ASME,  for example, position is essential for PQR, Product form etc. 

On Thu, 10 May 2018 5:29 pm 'wilfred kojo' via Materials & Welding, <materials-welding@googlegroups.com> wrote:
Hi,
It is true that inter pass temperature is measured after the pass (just before the commencement of subsequent pass) but why should it be controlled?
It's not measured because of previous pass but subsequent pass because it serves as preheat for subsequent pass which also control the cooling rate and mechanical properties.

On ‎Thursday‎, ‎10‎ ‎May‎ ‎2018‎ ‎10‎:‎36‎:‎16‎ ‎WAT, 'wilfred kojo' via Materials & Welding <materials-welding@googlegroups.com> wrote:


Hello Experts,
I think something is wrong here, we are interpreting code without understanding the background and the intent of clause requirements.
What is the difference between preheat temperature and inter pass temperature?
The preheat temperature is for first pass for the commencement of welding.
The inter pass temperature is the preheat temperature of the subsequent weld that why once PQR is qualified, the minimum preheat temperature also become the minimum inter pass temperature. In the same way maximum inter pass temperature also become the maximum preheat temperature qualified.
If the inter pass temperature of 110 deg. did not affect the mechanical properties of subsequent weld negatively why will the preheat of 110 deg.
Note minimum preheat temperature is essential variable while the maximum inter pass/preheat temperature is supplementary essential (only applicable when impact property is essential).
The maximum inter pass temperature is applicable because at higher inter pass or preheat temperature cooling rate will be low which lead to grain growth (the same reason why heat input is also supplementary essential variable). The higher the grain size the lower the impact property. 

On ‎Thursday‎, ‎10‎ ‎May‎ ‎2018‎ ‎05‎:‎41‎:‎03‎ ‎WAT, Ramesh <rameshkannandevaraj@gmail.com> wrote:


Hi

 

Practically your PQR was not preheated. It's room temperature and it was recorded as 30 Deg C.  but your WPS indicates preheat 110 Deg C !!! how is this acceptable when code does not allow to increase more than 56 Deg C from your PQR,

 

i.e. 30+56 is maximum allowed in WPS. So u have to restrict up to 86 Deg C NOT 110 Deg C

 

in case of interpass , your PQR recorded 173 Deg C, so 173+56 is maximum allowed in WPS i.e. 229 Deg C

 

In your case , preheat temperature is mentioned wrong i.e. 110 Deg C instead of 86 Deg C which is not acceptable. IP temperature mentioned / restricted 220 Deg C  which is OK.


Thanks and Regards


Rameshkannan Devaraj

M.Tech in Welding Engineering


"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"



On Thu, May 10, 2018 at 9:13 AM 'Rajnish Dixit' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Hi,
Please check respective WPS and refer the recorded maximum inter pass temperature. The condition is applicable if there will be increment of more than 56 deg Celsius in recorded/qualified inter pass temperature.

Thanks,
Warm Regards,

Rajnish Dixit
Lead - QA-QC/QMS/Welding/NDT/Inspection
+91 972 4200 357

On Wed, May 9, 2018 at 18:11, harish katesia
hello,

The subject under discussion is Max. preheat..It is 173 °c 

( Preheat/Interpass Temperature
7) An increase of more than 100°F [56°C] in the maximum preheat or interpass temperature qualified ) 

Max. preheat = Interpass temperature...

So anything between 30°c to 173°c is ok.

On Tue 8 May, 2018, 7:27 PM 'james gerald' via Materials & Welding, <materials-welding@googlegroups.com> wrote:
Moreover though maximum Interpass temperature controls the Austenitic Grain size and thus the Charpy values and Preheat controls the Temperature between 800-500 degC , but under ideal conditions using ASME Materials.

But below also have a effect

Chemical comp, method of maufacture, product form, Hardness, strength, Heat Treatment, microstructure, uniformity, homogenity, Grain size etc.. which are mostly controlled in the ASME Materials since its low temperature properties are controlled whereas material used in AWS D 1.1 have a effect.

Thanks & Regards

J.Gerald Jayakumar

0091-9344954677



On Tuesday, May 8, 2018, 1:10:17 PM GMT+4, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:


In ASME, % carbon is restricted to max 0.35%, where as in AWS it is more and properties will be deteriorated if use higher Pre Heat than qualified. That is why it is restricted.


THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Tue, May 8, 2018 at 1:03 PM, George Dilintas <dilintas@gmail.com> wrote:
in ASME IX also the increase is only for the interpass temperature and the decrease for the preheat.
The increase of interpass is a supplementary essential variable
the decrease of preheat is an essential one

2018-05-02 6:54 GMT+03:00 N VENKATESWARA PRASAD <weldengr.velosi@gmail.com>:
Dear Experts,

We have received a comment on Increase in Preheat temperature greater than 56°C is essential variable as per AWS D.1 from our client.

My interpretation is the increase in 56°C is applicable only for inter pass temperature.  The details are as given below. 

 

PQR   Test coupon thickness        :  30 mm

PQR   Preheat temperature          :  30°C

PQR Inter pass temperature        :  173°C

 

Job Thickness                                   : > 38 mm  to 65 mm  ( As per Table 3.3)

Preheat temperature                    :  110°C

Inter pass temperature                 :  220°C

MDMT                                                :  -40 °C

 

As per AWS D 1.1  Table 4.6  Point no. 7   an increase more than 56°C in max preheat or interpass temperature is essential variable  for CVN testing applications.

 

Based on the above clause, the client is insisting that the Qualified Range for  thickness in WPS shall be restricted to 38 mm as the preheat is increased from 30°C to 110°C which is not acceptable .

 

Please provide me if you any interpretation on it from AWS.

Regards

Prasad

--
https://materials-welding.blog spot.com/
https://www.linkedin.com/group s/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
Visit this group at https://groups.google.com/grou p/materials-welding.
For more options, visit https://groups.google.com/d/op tout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
Visit this group at https://groups.google.com/ group/materials-welding.
For more options, visit https://groups.google.com/d/ optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...