Re: [MW:23270] RE: 23260] Dissimilar Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)

The only issue in your case is to match the PWHT temperatures

P22 is a P-No 5A material, so the temperature range is 700 to 760 degC
P91 is a P-No 15E material, so the temperature range is 730 to 775 degC.
So you have to implement a strict control of the PWHT in order not to be lower than 730 and not higher than 760 deg C

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


Chirag Sandhane ---12/05/2015 08:49:22---Hi rushabh, There is no need of buttering with inconel182. U can use directly B3 for welding of this

From: Chirag Sandhane <chiragsandhane@gmail.com>
To: materials-welding@googlegroups.com
Date: 12/05/2015 08:49
Subject: Re: [MW:23268] RE: 23260] Dissimilar Joint between P22(2.25Cr-1Mo) to P91( 9Cr-1Mo-V)
Sent by: materials-welding@googlegroups.com





Hi rushabh,

There is no need of buttering with inconel182. U can use directly B3 for welding of this combination. If u refer PW 39 of section I, u can see notes given below in that table for this combination with B3 electrode min PWHT temp is 705.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at
http://groups.google.com/group/materials-welding.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/b59dbd4a-b18f-4b7b-b57e-155c4b6a2c83%40googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...