Skip to main content

Re: [MW:23267] Flux Trade Name for SAW

1. Who will perform the classification test?
Flux & wire manufacturer
2. While reviewing the PQR, does the vendor need to submit Classification records?

The marking on the boxes / cans and the MTR is an evidence for classification
3. If a PQR is qualified with Flux Trade Name "X", can this PQR be used to support another WPS where Flux Trade Name "Y" is mentioned without classification? Please note, X & Y are from different manufacturer.

No

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


Manas Ghosh ---11/05/2015 11:15:16---While qualifying a SAW Procedure as per ASME Sec IX, With respect to QW-404.9, the Flux Trade Name i

From: Manas Ghosh <m.k.ghosh1073@gmail.com>
To: materials-welding@googlegroups.com
Date: 11/05/2015 11:15
Subject: [MW:23265] Flux Trade Name for SAW
Sent by: materials-welding@googlegroups.com





While qualifying a SAW Procedure as per ASME Sec IX, With respect to QW-404.9, the Flux Trade Name is not an essential variable if the Flux Wire combination is Classified in ASME Sec II Part C (for A No 8, it is essential variable).

My queries are as follows
1. Who will perform the classification test?
2. While reviewing the PQR, does the vendor need to submit Classification records?
3. If a PQR is qualified with Flux Trade Name "X", can this PQR be used to support another WPS where Flux Trade Name "Y" is mentioned without classification? Please note, X & Y are from different manufacturer.

Please let me know your view. If you need further details, let me know.

Thanks and regards
Manas Ghosh

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at
http://groups.google.com/group/materials-welding.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/6b0fedef-fe83-4f74-9e72-110cddda9bae%40googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...