Skip to main content

Re: [MW:22970] Requirements Of PWHT for the Cross Country Pipe Lines - Reg

Hi as per yr qualified WPS you have to do the PWHT because this is as per code says as well as  ARAMCO .
 
So sorry there is no other option for u. 

On Wed, Mar 11, 2015 at 10:44 AM, 'Karthik' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Hi,
Since your WPS qu
 
Thanks & Regards,alified with PWHT, you can't use this for without PWHT jobs.
Since your construction code doesn't reqire PWHT you have 2 option.
01. Do new WPS/PQR without PWHT
02. If you don't want to prepare new, then follow as per your existing WPS (as your client said)

(Karthik)




On Friday, March 6, 2015 6:40 PM, Anup N K E <nkeanup@gmail.com> wrote:


Refer scope of work,  Isometric drawing and P & ID to find the applicable code.
Section 434.8.9 specifies about PWHT is ANSI B 31.4
Regards,
Anup
On 6 Mar 2015 08:59, "'mv_srinivasan' via Materials & Welding" <materials-welding@googlegroups.com> wrote:
Sir,
which design code is used whether ASME 31.4  or ASME 31.8.


Sent from Samsung Mobile


-------- Original message --------
From: Amul Raj
Date:05/03/2015 11:58 (GMT+03:00)
To: materials-welding@googlegroups.com
Subject: [MW:22939] Requirements Of PWHT for the Cross Country Pipe Lines - Reg

Dear Experts,

We have done PQR with PWHT for the Material APL 5L Grade X60, and the coupon Size is 40 Inch & the Thickness is 38 mm with the Construction code application of API 1104 (Cross Country Pipe Line)

Based on the results we prepared WPS Also, But, As per API 1104 for 38.00 mm THK PWHT is not required 

Now The Aramco PID instructed to follow the WPS to do all the Joints PWHT

What is the remdy for this & hat should we do 

Kindly drop your advise 


Thanks & Warm Regards,

Amul Raj T

QA/QC Welding 

Samsung Engg, KSA  



 




--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2f252b05-3866-481c-9fcf-2357a5f0c95e%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bx0ck71s8shh6put0pe6ceia.1425578687428%40email.android.com.
For more options, visit https://groups.google.com/d/optout.
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJsQutYVhgDnOXS2Cx2NuqVxUEtdST1CA3465R6j_3tQOudMUQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/322981801.3521275.1426063472120.JavaMail.yahoo%40mail.yahoo.com.

For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKh6c7d0t_AeAT1DzVzGrdHMTgk_1HEihN7HRephwQ1Q1NH3fg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...