[MW:23004] Re: ASME Sect IX-QW-405-Position Qualification Ranges

Hi Kunal
 
Addition of position is an essential variable for Hardfacing/ Corrosion resistant overlays. Please refer Table QW-256.1 for GTAW.
 
Thanks and Regards
Harikrishnan
On Wednesday, March 25, 2015 at 11:29:43 AM UTC+8, Kunal Patel wrote:
Dear friend,

Please refer ASME SEC-IX QW-203: Limit of Qualified Position for Procedure. Position is not essential variable for welding procedure except SAW welding process.

Kunal Patel
BVIPL

On Tuesday, 25 March 2014 14:18:59 UTC+5:30, Anban wrote:
Dear Experts

Position only a Supplementary essential variable (ie when CVN-Impact test required).

QW-405.2 A change from any position to the vertical position uphill progression. Vertical‐uphill progression
(e.g., 3G, 5G, or 6G position) qualifies for all positions. In uphill progression, a change from stringer bead to weave
bead. This variable does not apply when aWPS is qualified with a PWHT above the upper transformation temperature
or when an austenitic material is solution annealed after welding.

QW-405.4 (a) Qualification in the horizontal, vertical, or overhead position shall also qualify for the flat position. Qualification
in the horizontal fixed position, 5G, shall qualify for the flat, vertical, and overhead positions. Qualification in
the horizontal, vertical, and overhead positions shall qualify for all positions. Qualification in the inclined fixed position,
6G, shall qualify for all positions.

I'm looking at some of the WPS/PQRs received from Vendor. 
PQR state that Position Tested/Qualified- 1G
WPS state qualified for all groove and fillet positions?
CVN Tested at -30 deg C.

Based on QW-405.2 & QW-405.4- 1G does not qualify all positions.Only qualified for 1G & 1F.

Plls explain how "This variable does not apply when aWPS is qualified with a PWHT above the upper transformation temperature
or when an austenitic material is solution annealed after welding." relevant to Positions.


Pls shine some light on this. Thank You.



















































--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b28adefd-9dbd-46ae-a1f1-168fcb9b8e00%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...