Saturday, December 6, 2014

Re: [MW:22471] number of welding process in D1.1

Dear friend,

1 - Yes. You can, but it need WPS requalification. (see Table 4.7. item 18 - 2010 Ed.)

2 - The "ability to weld" and the "qualification" are two different things. It is probable that the welder could weld many types of joints in different positions and so on, but he has just 1 qualification. It means that he permits to weld just in the criteria of his qualification (and it doesn't mean that he is not able). So if your welder has ASME certificate and want to weld a part based on D1.1, he (or may be you) should prepare a new qualification based on D1.1.

Regards

On Fri, Dec 5, 2014 at 9:08 PM, Hamid Firoozi <h.firoozi61@gmail.com> wrote:
Hi All

1- Can we have more than one process in WPS based on D1.1 or not? please give me reference 

2 - Can we use one of the welding process from Section 9`s WPS for welder qualification, if welder should be qualified based on D1.1 ? (attention : test coupon will be test based on D1.1 criteria ) give me Guide line please.


Thanks everybody 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer

Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35354] Cast-iron welding

1. Preheat joint area(other area, cover with mineral wool). 2. ENiCi or ENiFe-CI. 3. stringer bead. 4. peening is to be done on weldmetal im...