Re: [MW:18948] P No.7 SA240 type 405 or 410S to Material P No.1 Group No.1 ( SA-516-60 )

410 to 516 gr 60------ 309 is best or 312
410 to 387gr5 ---------- NiCrFe3


On Mon, Oct 14, 2013 at 8:37 PM, Ramin Kondori <raminkondori@gmail.com> wrote:
Dear Piyush:

E309/ER309
E310/ER310
E312/ER312L

Use low carbon grades, keep dilution to minimum.
E310/ER310 gives you guaranteed results.
You can refer to delong or IIW diagrams to verify my suggestions.

Regards
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.kondori@petroyada.com
+98-2123592322
+98-9132150320



On Sat, Oct 12, 2013 at 6:15 PM, Octane Mac <octane.mac@gmail.com> wrote:
SA-240 Gr. 405/410S to SA-516 Gr. 60 /SA-387 Gr. 5 Cl. 2 > ER309 & E309
See attached from WeldPulse software.

Octane



On Wed, Oct 9, 2013 at 12:21 PM, Piyush <pankaj534@yahoo.com> wrote:
Dear Friends,
 
Could you please recommend AWS class for SMAW and GTAW welding consumable for P No.7 SA240 type 405 /410S to Material P No.1 Group No.1 ( SA-516-60 )  and   P No.7 SA240 type 405 or 410S to Material P No.5B Group No.1 ( SA-387 Gr. 5 Cl. 2 )     
 
Kind regards,
Piyush
      

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...