Re: [MW:18564] PWHT range for WPS

Dear Ram,

  the PWHT  temperature depend only to material grade. Your PQR is prepared for this range of temperature according material grade, so you can use it for the same material grade in production.

The time is according material thickness, you check the thickness qualified range and calculate the time as 1h per 01 inch thickness. (Refer to your construction code)

Regards.


2013/9/2 Ram Patel <rampatelindia2013@gmail.com>
Dear Experts

Can anybody explain me following about WPS & PQR as per ASME sex IX.

If my PQR qualifed with soaking temperature 630 deg. C to 650 deg. C and soaking time 2 hrs 30 minutes maximum, so my question is can WPS qualify for temperature range 600-620 deg.c or above 650 deg.c and soaking time 3 hrs or 2hrs.

My question for which temperature range or soaking time range I can use for WPS if my PQR qualified as per above mentioned PQR range ?.

Thanks in advance

Thanks
Ram

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
زكرياء غراب
GHRAB Zakaria
Jorf Lasfar Units 5&6 Power Plant construction Project
EA2C/ SDEM Entreprises
Site QA/QC Manager
Mobile : Morocco (+212) 6 61 07 00 11
             Tunisia (+216) 96 635 805



Yesterday is the pass, tomorrow is the future; and today? Today is the present, the gift: Enjoy it!

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:35346] Cast-iron welding

Any advice for cast iron welding Sent from Yahoo Mail for iPhone