Hi
My reply is not a direct answer to the query . However I would like to add that I have welded with 316 L and at weld metal got a FNo from 4 to 8. But the base metal too was ss316.
Thanks
Rgds
Rudolf
Sent from my iPhone
On 30 Jul, 2013, at 3:51 PM, Ramin Kondori <raminkondori@gmail.com> wrote:
> It seems that welder has used 316 filler metal
>
> On 7/30/13, Harikrishnan N S <hari.qaqc@gmail.com> wrote:
>> Dear Experts
>>
>> Recently I came across an issue of High Ferrite no. in the weld metal.
>>
>> Parent Metal : A 304L
>> Weld Metal : 308L
>> Welding Process : GTAW
>>
>> The affected area is only a quarter portion (3'o clock to 6'o clock
>> position) of the 30" pipe where ferrite no has been observed as over 21 FN.
>>
>> and PMI has shown 1.57% of Mo.
>>
>> Please give your valuable comments and rectification measures for this.
>> Refer the attached photos for clarity.
>>
>> Thanks and Regards
>> Harikrishnan
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>> ---
>> You received this message because you are subscribed to the Google Groups
>> "Materials & Welding" group.
>> To unsubscribe from this group and stop receiving emails from it, send an
>> email to materials-welding+unsubscribe@googlegroups.com.
>> For more options, visit https://groups.google.com/groups/opt_out.
>
>
> --
> *Ramin Kondori*
> *Sr. QA/QC Engineer
> *
> *SINOPEC*
>
> r.kondori@petroyada.com
> +98-2123592322
> +98-9132150320
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
My reply is not a direct answer to the query . However I would like to add that I have welded with 316 L and at weld metal got a FNo from 4 to 8. But the base metal too was ss316.
Thanks
Rgds
Rudolf
Sent from my iPhone
On 30 Jul, 2013, at 3:51 PM, Ramin Kondori <raminkondori@gmail.com> wrote:
> It seems that welder has used 316 filler metal
>
> On 7/30/13, Harikrishnan N S <hari.qaqc@gmail.com> wrote:
>> Dear Experts
>>
>> Recently I came across an issue of High Ferrite no. in the weld metal.
>>
>> Parent Metal : A 304L
>> Weld Metal : 308L
>> Welding Process : GTAW
>>
>> The affected area is only a quarter portion (3'o clock to 6'o clock
>> position) of the 30" pipe where ferrite no has been observed as over 21 FN.
>>
>> and PMI has shown 1.57% of Mo.
>>
>> Please give your valuable comments and rectification measures for this.
>> Refer the attached photos for clarity.
>>
>> Thanks and Regards
>> Harikrishnan
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>> ---
>> You received this message because you are subscribed to the Google Groups
>> "Materials & Welding" group.
>> To unsubscribe from this group and stop receiving emails from it, send an
>> email to materials-welding+unsubscribe@googlegroups.com.
>> For more options, visit https://groups.google.com/groups/opt_out.
>
>
> --
> *Ramin Kondori*
> *Sr. QA/QC Engineer
> *
> *SINOPEC*
>
> r.kondori@petroyada.com
> +98-2123592322
> +98-9132150320
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
Comments