Re: [MW:14764] Impact test qualification requirement for WPS/PQR

Dear Asad Azmi,

PQR 2 can be used to deposit 21mm thick weld if other essential and supplementary essential variables are same as PQR 1, since "T limits impact" (QW-403.6) has limitation only on min. thickness qualified.

Regards
Gogulu Kumar 

On Wed, Mar 14, 2012 at 4:01 PM, asad azmi <azmiasadayub@gmail.com> wrote:
Dear All,
 
Greetings.
 
A vessel is being fabricated as per ASME SEC VIII DIV 1.
 
Vessel material is SA 387 GR 12 CL2, 65 THK. MDMT is   -18 DEG CELCIUS.
 
Approved WPS is supported by  2 PQR  detailed as below --
 
PQR 1
 
Test coupon thickness - 40 mm ,
Welding process used - GTAW + SMAW + SAW ,
Weld deposit by SMAW  Process is 19 mm.
Weld deposited by SMAW  is impact tested at   0 deg celcius.
 
PQR 2
 
Test coupon thickness - 10 mm ,
Welding process used - GTAW + SMAW ,
Weld deposit by SMAW  Process is 8 mm.
Weld deposited by SMAW  is impact tested at    - 18 deg celcius.
 
Whether  PQR  2 can be used for SMAW  Process to deposit  21 mm weld in a weld groove of 65 mm in depth .( for closing seam of shell to dished head & nozzle to dished  head weld seam)
 
Please advice. please give ASME SEC IX Reference.
 
Thanks & Regards
 
Asad Azmi
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Regards
Gogulu Kumar
+919765804701


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...