Dear Sirs,
The project requirements perhaps depend on design parameter but this has nothing to do with the requirements mentioned in material specification.
EN 10025 chapter 7.4.2.4 mentions that when Charpy impact tests need to be proven by tests on the materials delivered it should be agreed in front (purchase order) for material grades JR (Supplement requirement 9).
For material grades J0 it's a standard requirement so every certificate should mention results of impact test (req. >27J at 0 °C) for this specific heat number and therefore material delivered with certificates without mentioning impact values should be rejected.
Met vriendelijke groeten / Best Regards
Herman Pieper
Pieper Quality Support & Inspection
Phone: +31 (0)521 380083
Fax: +31 (0)84 7539225
Cell: +31 (0)6 51691215
Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens Vino Varghese
Verzonden: zaterdag 10 september 2011 13:50
Aan: materials-welding@googlegroups.com
Onderwerp: Re: [MW:12413] Impact test requirement for JO and JR grades in structural fabrication.
Dear Arvinda,
The Impact requirement depends on Design Parameter of the Project.
Please check whether Contract / Project Spec / Service calls for impact.
Thanks & Regards
Vino-Doha
_________________________________________________________________________
On Sat, Sep 10, 2011 at 10:40 AM, arvinda shan <arvindashan@gmail.com> wrote:
Dear Experts,
For crosshead installation in jetty project, the following materials (37mm) are used.
Road way - S355JO
Crosshead - S355JR & S275JR
Pipe track - S355JR
As per European structural steel standard EN10025 , for JR grade, Longitudinal charpy V-notch impacts 27J @20 degrees and for JO grade, Longitudinal charpy V-notch impacts 27J @ 0 degrees.
We received materials mill certificates w/o impact test.
My question is whether impact is mandatory for above grades or any criteria of thickness as per EN10025? Please mention with reference codes.
Your valuable suggestions are appreciated.
Regards
arvinda
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment