Re: [MW:7230] Heat treatment Butt joint of SA-210 Gr.A1 and SA-312 TP 304H

Dear Shinde,
 
The carbon content in TP 304H is 0.04% to  0.10%. When we heat (above 500degC) unstabilized austenitic stainless steel that have carbon content more than 0.03%,its intergranular corrosion resistance decreases significantly. This is because of precipitation of chromium carbides in grain boundries (i.e. Sensitization) while  slow cooling in the range of 450 to 650 degC.
 
As per ASME Sec VIII Div I, PWHT for SA 210 GrA-1 (P.No. 1 & Gr. No.1) shall be carried as follows:
Heating&Cooling rate: 100degC/Hr
Soaking Temperature: 595degC
 
So PWHT temperature may lead to sensitization of 304H. So it is better to butter the carbon steel with stabilized stainless steel electrode like E309Nb or low carbon fillers like ER309L/LMo and then do the PWHT. Finally the weld the buttering to the TP304H using E/ER 308H.
 
Or else, use SA 312 TP 347H/321H tubes & weld it with E/ER 347H to carbon steel and straight away do the PWHT as above.
 
Because TP 321 is titanium stabilised and TP 347 is niobium stablised stainless steel. Ti an Nb is having more affinity towards carbon. Titanium carbide/ Niobium carbide will form instead of Chromium carbide. Hence sensitization can be avoided.
 


 
On Sun, Sep 26, 2010 at 3:17 PM, agstes <agstes@gmail.com> wrote:
Dear Sudharsan S,
 
This particular joint is one of the joint from the heat recovery steam generator (unfired) constructed as per ASME Section VIII Div.1. As per UW-2 (c) this particular steam generator needs to be heat treated.
Thickness involved 12.7 mm.
In my opinion there should not be any problem for the SS material like carbide precipitation.
Please suggest the heat cycle.
 
Thanks in advance.
Regards
Shinde
----- Original Message -----
Sent: Sunday, September 26, 2010 1:55 PM
Subject: Re: [MW:7199] Heat treatment Butt joint of SA-210 Gr.A1 and SA-312 TP 304H

Shinde,
 
SA 210 Gr A1 is a seamless medium carbon (0.27% max) steel tubes. If you weld this to SA 312 TP 304H (18% Cr 8% Ni) with fully austenitic electrode like AWS E/ER 309LMo, from metallurgical point of view , there is no need for PWHT.
 
Can you just tell me why you need PWHT, is it from process point of view or for any other reason? What is the thickness as well.
 
On Fri, Sep 24, 2010 at 6:25 PM, agstes <agstes@gmail.com> wrote:
Dear All,
 
I want to know the post weld heat treatment procedure/cycle for the butt joint of SA-210 Gr.A1 (P1) and SA-312 TP 304H (P8).
 
Thanks in advance.
 
Shinde A.G.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...