Skip to main content

Re: [MW:6767] PWHT of dis-similar materials

Why do you have to keep the hydrotest caps on after hydrotest? I would advise you to remove the caps and then do the PWHT.

Johnson Madukayil

On Sun, Aug 29, 2010 at 11:23 AM, Safa Özhan <safaozhan@gmail.com> wrote:
Dear All,

I think we've got a really serious problem regarding PWHT of dissimilar
materials.

In some of our in-house applications, we have to weld hydro test caps on
open ends' of pipe-spools in order to hydro test them.
After welding of caps are completed, we heat treat the spools together with
(most of the time caps made of dissimilar material, mostly CS Caps because
of cheapness) Hydro-Test caps. Even though, thickness of these hydro test
caps are calculated as per related code, one of our concern starts because
of the effects of excessive heat treatment on hydro test caps. Because; as
per codes, allowable stress values should be chosen in accordance with the
hydro test temperature which should be lower because of excessive PWHT, but
how much ? Are there any codes explaining this situation ? Does any member
has experienced same kind of problem ?

Other concerning point is the service life of that work piece.  Even though
the caps work properly after PWHT, then the question should be how many
times we can use that caps in our other hydro tests, of course safely.

The main problem indeed is, are there any approach which can assume/predict
the material properties (Especially reduction in durability.) after PWHT
depending of PWHT parameters ?

It would be highly appreciated if some of you can address a code with a
working example of solution.

In order to visualize the problem pls see below example of the concerning
situation;

- Material of spool is P91 and the cap's is CS.
- PWHT temp  : 730 C
- PWHT duration : 1 hr.

How can we calculate the reduction in durability ?

Thanks for your time,

Regards,

Safa


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...