Obviously you have to use E9018-X classification according to your PSL .Many specification say the strength level should be matched .In case of pipeline we have see the Y.S also Refer DNV –OS-F101 specification

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of dinesh verma
Sent: 23 August 2010 20:49
To: materials-welding@googlegroups.com
Subject: Re: Re: [MW:6661] ELECTRDOE STRENGHT REQUIRMNET FOR PLATE GR65

 


pl clarify why E8018 MIN TENSILE 80,000 PSI ELECTODE IS BEING USED IN MANY OF THE LINE PIPE WELDING OF GRADE API 5L X 70 WHOSE MIN TENSILE IS 82,000 PSI
REGARDS
DINESH
On Mon, 23 Aug 2010 21:57:53 +0530 wrote
>Sujeeth,
              In all PQR testing as per ASME SEC-IX requires Tensile strength only .How can you calculate based on Yield strength.
 
vaithiyanathan

 
On 8/22/10, Sujeet Sangle wrote:



We should select the consumable with the YS and no TS properties .
 
Regards,
 
Sujeet
 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of B.Vaithiyanathan

Sent: Sunday, August 22, 2010 5:56 PM
To: materials-welding@googlegroups.com

Subject: Re: [MW:6625] ELECTRDOE STRENGHT REQUIRMNET FOR PLATE GR65

 

Always the welding electrode should meet Base material strength .By this way the electorde slection should be F7A0 .

 

Regards,

Vaithiyanathan,

 



 

On 8/22/10, Syed Moin wrote:


Dear Members,
Appreciate if you could provide me some information on the issue, During a PQR, manufacturer has used electrode F6A0-EM12 to weld plates A516 Gr. 65, welding procedure is SAW. Below is the comparison, between the tensile strength of the electrode,

comparison table                               
        WELDING FLUX F6A0       PLATE   flux certificate(see attachment)        Strength of the plate material 

        REFER TO SFA 5.17       ASTM A516, GR65 test result     Test Result    
        Tensile Tensile tensile         tensile

        60,000~80,000 psi       65000~85,000 psi         72289 psi (500MPa)     68875 psi (475 Mpa)    
                                       
Our client says that the selected electrode is not suitable for Gr. 65c plates. Is it correct?

They say that the electrode shall be selected considering the minimum strength ( for this electrode minimum strength is 60, 000 PSI), and therefore it is not suitable for a plate with minimum strength value equal to 65000 PSI .

As you can see in the above  table tensile test value for the electrode is 72289 PSI, but still the client is not ready to accept the use of this electrode.

Please advise.
Regardsa
MS
 

______________________________________________________
CONFIDENTIALITY NOTICE: This electronic mail transmission may contain information that is confidential, privileged, proprietary, or otherwise legally exempt from disclosure and is intended only for the use of the recipient named above. We do not waive confidentiality in the event this mail was transmitted wrongly. If you have received this communication in error, and are not the intended recipient, you are hereby notified that you are prohibited from reading, printing, copying, or disseminating this message, any part of it, or any of the attachments it may carry. If you have received this message in error, please destroy all electronic and paper copies and notify the sender immediately of the inadvertent transmission. We would like to advise you that we would not waive any of our privilege for taking action against you in the event the confidentiality of this message has been compromised. Thank you for your cooperation

________________
This email has been scanned by the MessageLabs Email Security System.
For more information please visit http://www.messagelabs.com/email

______________________________________________________________________
 
--
To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
With Best Regards

B.Vaithiyanathan
--
To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Disclaimer: If you are not the intended recipient, you must not copy, distribute or use it for any purpose, nor disclose its contents to any other person. Any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the company. The company will not accept any liability in respect of such communication, and the employee responsible will be personally liable for any damages or liability arising from, but not limited to, defamatory statements, infringement of copyright or any other legal right. Please delete the email and notify the sender immediately if you receive this in error.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
With Best Regards

B.Vaithiyanathan



--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...