Hi Luis,

The material is 2.25Cr-1Mo steel (P 5A Gr 1)  in the shape of casting. What' the other material to be welded? A rule of thumb could be :-

  • A 217 Gr WC9 to P4 material-- Use P4 matching electrode for buttering, e.g-E 8018/16 B2 or E-7018B2 or GTAW filler of equivalent specification. You may use E-9018B3 or 8018B3L also, in that case buttering sequence may not be needed.
 
  • A 217 Gr WC9 to S.S- Use Inconel-182(E NiCrFe-3) or matching GTAW filler(ERNiCr-3) for buttering.PWHT the buttered area and   P5 steel as recommended by design code followed by welding to P8 without further PWHT.
Note the above guidelines are only generalized rule. Buttering sequences and welding electrodes to be used would depend on what material gets welded to A 217 Gr WC9 and the code or specification requirements.
 
Note the  precautions and welding parameters to be followed for buttering shall be identical to a groove  weld.
 
Thanks.
 
Pradip Goswami,P.Eng.
Welding & Metallurgical Engineer/Specialist
Ontario Power Generation Inc.
Email-pgoswami@sympatico.ca,
pgoswami@quickclic.net

-----Original Message-----
From: materials-welding@googlegroups.com [
mailto:materials-welding@googlegroups.com] On Behalf Of Luis Carlos
Sent: Monday, August 30, 2010 12:37 PM
To: Materials & Welding
Subject: [MW:6788] A 217 Gr WC9

Hello,

Could someone tell me please what is the best filler metal to make a buttering over A-217 Gr WC9 base metal.

Are there special recommendations?

I will appreciate answers!

Luis Carlos


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...