Please note that for LTCS piping, it is mandatory to comply the requirements of Table 323.2.1 (Welding procedure qualification) and Table 323.3.1 (Weld production testing) like pressure vessels as per Sec. VIII Div. 1.

 

For your case, please refer to Note -2 of Table 323.2.2, which indicates that production weld testing can be preformed as a part of welding procedure qualification, provided it shall meet all the requirements as stated in Table 323.3.1 including thickness limitations i.e. T/2 to T+6mm.

 

You need to segregate the thickness ranges involved for LTCS piping and accordingly you need to qualify or support the existing PQR to meet the above thickness limitation.

 

Regards,

 

L. Prabhu kumar,

Sr. Principal Engineer,

 

Equipments & Materials Dept.,

Saipem India Projects Limited,

Nungambakkam High Road, Chennai - 600 034, India.

Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,

Mobile Ph. No.: +91 9003010978.


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manpreet
Sent: Wednesday, May 26, 2010 12:02 PM
To: materials-welding@googlegroups.com
Subject: [MW:5253] Thickness for impact testing

 

Dear All

My case is


Material- Low carbon steel
Applicable code: ASME B 31.3

According to ASME IX QW-403.6, the minimum base metal thickness qulified is the thickness of test coupon T or 0.625" (5/8"), whichever is less. That is 0.5". Therefore, the thickness range 0.25"-0.5" is not qualified.

But the vendor pointed out the the qualified thickness range can based on fabrication code B31.3 Table 323.3.1 which indicates that qualifed thickness range is T/2 to T+0.25".

In this case, what is the minimum qulified thickness: 0.25" or 0.5"? Please advise.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

 




-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or 
entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged 
information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution 
or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If 
you have received this communication in error, please notify us immediately by responding to this email and then 
delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete 
transmission of the information contained in this communication nor for any delay in its receipt. 
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...