Skip to main content

Re: [MW:4529] RE: 4520] RE: 4518] Re: tests for checking welding quality of Duplex SS weld

In addition to Ferrite control by ferrite scope for root pass and subsequent passes ,even required weld colour shade may also be used as a guideline for checking the quality of duplex .super duplex , 6Mo materilas.
Regards,
Francis Lobo
----- Original Message -----
From: Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com>
To: materials-welding@googlegroups.com
Sent: Wed, 10 Mar 2010 12:59:05 +0530 (IST)
Subject: [MW:4521] RE: 4520] RE: 4518] Re: tests for checking welding quality of Duplex SS weld


ISO 5817, which gives guidelines on acceptance levels for various defects in welded joints.
EN 288 and ASME IX, which describe the approval of welding procedures.
However, duplex steels are used in applications where the strength and corrosion requirements are very severe. There is thus every reason to be extra careful from beginning to end. Welding oxide, spatter,
striking scars and grinding scars must be removed to achieve the correct corrosion resistance. For the best fatigue resistance, the weld surface must be even with no sharp edges.
Nondestructive testing is an integral part of the examination of welded joints. Suitable methods are visual inspection, penetrant testing (PT), radiographic testing (RT), ultrasound testing (UT) and ferrite content measurement (ISO 8249 and AWS A4.2) using a "ferritescope". In ultrasound testing, it is important that surfaces are ground flat so that defects such as pores and cracks can be reliably detected.

-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Tran Van Vuong
Sent: Wednesday, March 10, 2010 12:33 PM
To: materials-welding@googlegroups.com
Subject: [MW:4520] RE: 4518] Re: tests for checking welding quality of Duplex SS weld

Dear,

X-ray test is preferred. EN 1435/ EN 25817, UT may be applied EN 1714/ EN
1712 (Level 2 or B)

TRAN VAN VUONG

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of hongkythai
Sent: Wednesday, March 10, 2010 1:55 PM
To: Materials & Welding
Subject: [MW:4518] Re: tests for checking welding quality of Duplex SS weld

Hi Pankaj,
You can find the European standrad is BS EN 287 and BS EN 288 for checking the welding quality of Duplex stainless steel.

Brg,

Hong Ky Thai
QUATEST3 inspector, Vietnam

On Mar 10, 1:29 pm, pankaj.jo...@in.transport.bombardier.com wrote:
> Hi,
>
> Can anybody suggest what tests must be conducted to check welding
> quality of Duplex SS.
> Is there any European standard for these tests details.
>
> BR,
>
> Pankaj Johri,   GradIEAust,

Filtered by Hosted Filtering


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

click for exclusive coverage on the New Bajaj Pulsar 220 the fastest Indian bike
http://www.zigwheels.com/Features/Bajaj-Pulsar-220-DTSi-Special-Coverage/Pulsar_20090623-1-1

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...